Steel heat treatment chart
Hardening temperature, quench, tempering range and typical hardness for the steels knife makers, blacksmiths and machinists use most. Pick a grade for its composition, critical temperatures and sources.
Carbon steels
| Grade | Austenitize °C | Austenitize °F | Quench | Temper °C | Typical hardness |
|---|---|---|---|---|---|
| 1018 | 900 to 925 | 1650 to 1695 | Oil or water after carburizing | 150 to 200 | Case about 58 to 62 HRC, core stays soft |
| 1045 | 815 to 845 | 1500 to 1555 | Water or brine, oil for thin sections | 315 to 595 | About 55 HRC as quenched at the surface, 20 to 30 HRC after machinery tempers |
| 1060 | 800 to 830 | 1470 to 1525 | Medium-fast oil | 175 to 370 | 56 to 58 HRC with a 200 C temper, lower for springs |
| 1075 | 800 to 830 | 1470 to 1525 | Fast oil | 175 to 260 | 55 to 58 HRC after a 200 C temper |
| 1080 | 800 to 830 | 1470 to 1525 | Fast oil | 175 to 260 | 56 to 59 HRC after a 200 C temper |
| 1084 | 800 to 830 | 1470 to 1525 | Fast oil | 175 to 230 | 57 to 60 HRC after a 190 to 200 C temper |
| 1095 | 790 to 815 | 1455 to 1500 | Very fast oil | 175 to 230 | 58 to 62 HRC after a 190 C temper |
| 15N20 | 790 to 815 | 1455 to 1500 | Fast oil | 175 to 230 | 57 to 60 HRC after a 200 C temper |
| 26C3 | 790 to 815 | 1455 to 1500 | Fast oil, brine only on thin blades by experienced hands | 150 to 200 | 62 to 65 HRC after a low temper |
Alloy steels
| Grade | Austenitize °C | Austenitize °F | Quench | Temper °C | Typical hardness |
|---|---|---|---|---|---|
| 4130 | 855 to 885 | 1570 to 1625 | Oil, water for heavy sections | 400 to 565 | 28 to 36 HRC quenched and tempered |
| 4140 | 845 to 870 | 1555 to 1600 | Oil | 400 to 650 | About 54 to 59 HRC as quenched, 28 to 36 HRC after machinery tempers |
| 4340 | 815 to 845 | 1500 to 1555 | Oil | 200 to 650 | About 53 to 55 HRC as quenched, chosen temper sets the strength class |
| 5160 | 815 to 845 | 1500 to 1555 | Oil | 190 to 480 | 57 to 59 HRC at a 200 C temper for blades, 44 to 48 HRC at spring tempers |
| 6150 | 845 to 885 | 1555 to 1625 | Oil | 400 to 540 | 42 to 48 HRC at spring tempers |
| 8620 | 900 to 925 | 1650 to 1695 | Oil, direct or after reheating to about 815 to 845 C | 150 to 200 | Case 58 to 62 HRC, core roughly 30 to 40 HRC |
| 9260 | 815 to 870 | 1500 to 1600 | Oil | 190 to 480 | 57 to 59 HRC at a 200 C temper, 45 to 50 HRC at spring tempers |
| 9310 | 900 to 925 | 1650 to 1695 | Oil | 150 to 200 | Case 58 to 62 HRC, core about 34 to 42 HRC |
| 52100 | 840 to 860 | 1545 to 1580 | Oil | 160 to 230 | 58 to 64 HRC depending on temper |
| 80CrV2 | 800 to 840 | 1470 to 1545 | Fast oil | 175 to 230 | 56 to 60 HRC after a 200 C temper |
| 300M | 855 to 885 | 1570 to 1625 | Oil | 285 to 315 | 52 to 55 HRC, tensile strength around 1900 to 2000 MPa |
Tool steels
| Grade | Austenitize °C | Austenitize °F | Quench | Temper °C | Typical hardness |
|---|---|---|---|---|---|
| W1 | 760 to 815 | 1400 to 1500 | Water or brine, interrupted for thin sections | 150 to 230 | 58 to 64 HRC at the surface |
| O1 | 790 to 815 | 1455 to 1500 | Oil | 150 to 260 | 57 to 64 HRC depending on temper |
| A2 | 925 to 980 | 1695 to 1795 | Still air or aluminium plates | 175 to 230 | 57 to 62 HRC |
| D2 | 1000 to 1030 | 1830 to 1885 | Air, plates, or vacuum gas quench | 200 to 530 | 59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C |
| S7 | 925 to 955 | 1695 to 1750 | Air up to about 60 mm, otherwise interrupted oil | 205 to 540 | 54 to 57 HRC at a 205 C temper |
| H13 | 995 to 1040 | 1825 to 1905 | Vacuum gas quench or still air | 550 to 620 | 44 to 52 HRC after double or triple tempering |
| M2 | 1180 to 1220 | 2155 to 2230 | Salt bath, oil, or vacuum gas quench | 540 to 570 | 63 to 66 HRC after triple tempering |
Stainless steels
| Grade | Austenitize °C | Austenitize °F | Quench | Temper °C | Typical hardness |
|---|---|---|---|---|---|
| 420 | 980 to 1035 | 1795 to 1895 | Air or oil | 150 to 370 | 48 to 53 HRC |
| 440C | 1010 to 1065 | 1850 to 1950 | Air, plates, or oil | 150 to 230 | 57 to 60 HRC |
| AEB-L | 1050 to 1080 | 1920 to 1975 | Aluminium plates with forced air, then cold treatment | 150 to 200 | 60 to 63 HRC with cold treatment |
| 154CM | 1050 to 1095 | 1920 to 2005 | Plates or oil, then cold treatment | 150 to 230 | 59 to 62 HRC |
| MagnaCut | 1065 to 1120 | 1950 to 2050 | Aluminium plates, then cold treatment | 150 to 175 | 60 to 64 HRC |
Steels compared
- 1084 vs 1095
- 1075 vs 1084
- 1080 vs 1084
- 1095 vs O1
- 1095 vs W1
- 1095 vs 26C3
- 1084 vs 15N20
- 1084 vs 80CrV2
- 5160 vs 80CrV2
- 1095 vs 5160
- 5160 vs 9260
- 5160 vs 6150
- 1095 vs 52100
- 52100 vs O1
- 80CrV2 vs 52100
- O1 vs A2
- A2 vs D2
- O1 vs D2
- O1 vs W1
- A2 vs S7
- D2 vs S7
- H13 vs S7
- D2 vs M2
- D2 vs MagnaCut
- AEB-L vs MagnaCut
- 154CM vs MagnaCut
- 154CM vs 440C
- 440C vs AEB-L
- 420 vs 440C
- 154CM vs AEB-L
- 4130 vs 4140
- 4140 vs 4340
- 1045 vs 4140
- 1018 vs 1045
- 1045 vs 1060
- 300M vs 4340
- 8620 vs 9310
- 1018 vs 8620
- 4140 vs 8620
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
This chart, plus a calculator for any composition.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat