4340 steel heat treatment

The deep-hardening high-strength steel for crankshafts, gears and aircraft parts. Strong and tough at once. Typical practice for AISI 4340: austenitize at 815 to 845 °C (1500 to 1555 °F), quench (oil), then temper at 200 to 650 °C (390 to 1200 °F).

Austenitize
815 to 845 °C
1500 to 1555 °F
Temper
200 to 650 °C
390 to 1200 °F
Quench
Oil
Typical hardness
About 53 to 55 HRC as quenched, chosen temper sets the strength class

Hardens through in large sections thanks to nickel plus chromium plus molybdenum. Avoid tempering in the embrittlement window around 260 to 370 C.

Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

4340 chemical composition

4340 chemical composition in weight per cent
ElementSymbolWeight %
CarbonC0.38 to 0.43
ManganeseMn0.6 to 0.8
SiliconSi0.15 to 0.35
NickelNi1.65 to 2
ChromiumCr0.7 to 0.9
MolybdenumMo0.2 to 0.3

These are the limits of the standard's chemical range. Ni-Cr-Mo alloy steel. Also known as: 34CrNiMo6 (near), 1.6582 (near), En24, 817M40, SNCM439.

4340 critical temperatures

Estimated critical temperatures for 4340
TemperatureWhat it meansEstimateEquation
Ac1Lower critical temperatureabout 705 °C (1302 °F)Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W
Ac3Upper critical temperatureabout 772 °C (1422 °F)Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W
MsMartensite startabout 303 °C (577 °F)Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo

Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.

Questions

What temperature do you harden 4340 steel at?
Austenitize 4340 at 815 to 845 °C (1500 to 1555 °F), then quench: oil. This is typical published practice; section size and furnace accuracy shift the right number.
What temperature do you temper 4340 at?
Temper 4340 at 200 to 650 °C (390 to 1200 °F). Typical hardness: about 53 to 55 HRC as quenched, chosen temper sets the strength class.
What do you quench 4340 steel in?
Oil. Hardens through in large sections thanks to nickel plus chromium plus molybdenum. Avoid tempering in the embrittlement window around 260 to 370 C.
What is 4340 steel equivalent to?
Other designations for 4340, or for its nearest equivalent where marked "near": 34CrNiMo6 (near), 1.6582 (near), En24, 817M40, SNCM439. Check the chemistry on your supplier's datasheet before treating them as the same steel.

Enter your own composition and get the numbers, with sources.