W1 steel heat treatment
The old-school tool steel: plain high carbon, water quenched, hard skin over a tough core. Typical practice for W1: austenitize at 760 to 815 °C (1400 to 1500 °F), quench (water or brine, interrupted for thin sections), then temper at 150 to 230 °C (300 to 445 °F).
- Austenitize
- 760 to 815 °C
- 1400 to 1500 °F
- Temper
- 150 to 230 °C
- 300 to 445 °F
- Quench
- Water or brine, interrupted for thin sections
- Typical hardness
- 58 to 64 HRC at the surface
The A681 specification spans carbon classes from 0.70 to 1.50; the values shown are a common cutlery class. Very shallow hardening, which is the feature: the core stays unhardened and tough.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
W1 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.95 to 1.1 |
| Manganese | Mn | 0.25 |
| Silicon | Si | 0.25 |
These are the producer's typical values, not a standard range. Water-hardening tool steel. Also known as: 1.1545 (near), SK85 to SK105 (near).
W1 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 728 °C (1342 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | Withheld | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 98 °C (208 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
W1 is hypereutectoid (carbon above about 0.8%), so it has no Ac3. The boundary that matters is Acm, where carbides dissolve, and the steel is normally hardened from between Ac1 and Acm.
Above about 0.8% carbon, normal hardening leaves some carbon locked in carbides. Less carbon is dissolved than the bulk analysis says, so the real Ms of W1 sits higher than this estimate.
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden W1 steel at?
- Austenitize W1 at 760 to 815 °C (1400 to 1500 °F), then quench: water or brine, interrupted for thin sections. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper W1 at?
- Temper W1 at 150 to 230 °C (300 to 445 °F). Typical hardness: 58 to 64 HRC at the surface.
- What do you quench W1 steel in?
- Water or brine, interrupted for thin sections. The A681 specification spans carbon classes from 0.70 to 1.50; the values shown are a common cutlery class. Very shallow hardening, which is the feature: the core stays unhardened and tough.
- What is W1 steel equivalent to?
- Other designations for W1, or for its nearest equivalent where marked "near": 1.1545 (near), SK85 to SK105 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other tool steels
- O1Oil-hardening tool steel
- A2Air-hardening tool steel
- D2High-carbon high-chromium tool steel
- S7Shock-resisting tool steel
- H13Hot-work tool steel
- M2High-speed steel
Sources for this grade: ASTM A681 (carbon by class, typical class shown); Typical published practice.
Enter your own composition and get the numbers, with sources.