8620 steel heat treatment
The standard carburizing steel for gears: glass-hard case over a tough low-carbon core. Typical practice for AISI 8620: carburize at 900 to 925 °C (1650 to 1695 °F), quench (oil, direct or after reheating to about 815 to 845 C), then temper at 150 to 200 °C (300 to 390 °F).
- Carburize
- 900 to 925 °C
- 1650 to 1695 °F
- Temper
- 150 to 200 °C
- 300 to 390 °F
- Quench
- Oil, direct or after reheating to about 815 to 845 C
- Typical hardness
- Case 58 to 62 HRC, core roughly 30 to 40 HRC
Case depth is set by carburizing time and temperature, not by the quench. The alloy content keeps the core from collapsing under contact loads.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
8620 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.18 to 0.23 |
| Manganese | Mn | 0.7 to 0.9 |
| Silicon | Si | 0.15 to 0.35 |
| Nickel | Ni | 0.4 to 0.7 |
| Chromium | Cr | 0.4 to 0.6 |
| Molybdenum | Mo | 0.15 to 0.25 |
These are the limits of the standard's chemical range. Case-hardening alloy steel. Also known as: 21NiCrMo2, 1.6523, 805M20, SNCM220.
8620 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 721 °C (1330 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 827 °C (1521 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 411 °C (771 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you carburize 8620 steel at?
- Carburize 8620 at 900 to 925 °C (1650 to 1695 °F), then quench: oil, direct or after reheating to about 815 to 845 C. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 8620 at?
- Temper 8620 at 150 to 200 °C (300 to 390 °F). Typical hardness: case 58 to 62 HRC, core roughly 30 to 40 HRC.
- What do you quench 8620 steel in?
- Oil, direct or after reheating to about 815 to 845 C. Case depth is set by carburizing time and temperature, not by the quench. The alloy content keeps the core from collapsing under contact loads.
- What is 8620 steel equivalent to?
- Other designations for 8620, or for its nearest equivalent where marked "near": 21NiCrMo2, 1.6523, 805M20, SNCM220. Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other alloy steels
- 4130Cr-Mo alloy steel
- 4140Cr-Mo alloy steel
- 4340Ni-Cr-Mo alloy steel
- 5160Cr spring steel
- 6150Cr-V spring steel
- 9260Si-Mn spring steel
- 9310Case-hardening alloy steel
- 52100Bearing steel
- 80CrV2Cr-V high carbon steel
- 300MUltra-high-strength steel
Sources for this grade: SAE J404 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.