Skip to content

1045 vs 1060 steel

1045 (Medium-carbon steel). The workhorse medium-carbon steel for shafts, axles and machine parts, used quenched and tempered.

1060 (Medium-high carbon steel). A tough sword and spring carbon steel. Takes a good edge yet bends before it breaks.

How 1045 and 1060 differ

  • 1060 carries more carbon: 0.55 to 0.65% against 0.43 to 0.5% in 1045.
  • 1045 is austenitized hotter: 815 to 845 °C (1500 to 1555 °F) against 800 to 830 °C (1470 to 1525 °F) for 1060.
  • The quench differs. 1045: water or brine, oil for thin sections. 1060: medium-fast oil.

Side by side

1045 and 1060 compared
10451060
TypeMedium-carbon steelMedium-high carbon steel
Carbon (C), wt %0.43 to 0.50.55 to 0.65
Manganese (Mn), wt %0.6 to 0.90.6 to 0.9
Austenitize815 to 845 °C (1500 to 1555 °F)800 to 830 °C (1470 to 1525 °F)
QuenchWater or brine, oil for thin sectionsMedium-fast oil
Temper315 to 595 °C (600 to 1105 °F)175 to 370 °C (345 to 700 °F)
Typical hardnessAbout 55 HRC as quenched at the surface, 20 to 30 HRC after machinery tempers56 to 58 HRC with a 200 C temper, lower for springs
Ac1 (lower critical temperature)about 715 °C (1319 °F)about 715 °C (1319 °F)
Ac3 (upper critical temperature)about 772 °C (1421 °F)about 753 °C (1387 °F)
Ms (martensite start)about 320 °C (607 °F)about 262 °C (504 °F)

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

1045

Shallow hardening: heavy sections harden at the skin only. Water quenching risks distortion and cracks on sharp corners, so radius and pre-machine generously.

1060

A favorite for large blades because the lower carbon leaves more ductility than 1084 or 1095 at the same temper.

Questions

What is the difference between 1045 and 1060 steel?
1060 carries more carbon: 0.55 to 0.65% against 0.43 to 0.5% in 1045. 1045 is austenitized hotter: 815 to 845 °C (1500 to 1555 °F) against 800 to 830 °C (1470 to 1525 °F) for 1060.
Is 1045 or 1060 harder after heat treatment?
Typical hardness for 1045: about 55 HRC as quenched at the surface, 20 to 30 HRC after machinery tempers. For 1060: 56 to 58 HRC with a 200 C temper, lower for springs. The result depends on the temper you choose.
Can I heat treat 1045 and 1060 the same way?
No, each has its own recipe. 1045: austenitize at 815 to 845 °C, quench in water or brine, oil for thin sections, temper at 315 to 595 °C. 1060: austenitize at 800 to 830 °C, quench in medium-fast oil, temper at 175 to 370 °C.

Heat treatment numbers for your own steel, with sources.