1084 steel heat treatment
The classic beginner blade steel: eutectoid carbon, wide forgiving windows, clean results in a home shop. Typical practice for AISI 1084: austenitize at 800 to 830 °C (1470 to 1525 °F), quench (fast oil), then temper at 175 to 230 °C (345 to 445 °F).
- Austenitize
- 800 to 830 °C
- 1470 to 1525 °F
- Temper
- 175 to 230 °C
- 345 to 445 °F
- Quench
- Fast oil
- Typical hardness
- 57 to 60 HRC after a 190 to 200 C temper
At eutectoid carbon everything transforms cleanly with no excess carbide to manage. Normalize after forging, then harden from a low soak. Pattern-welds beautifully against 15N20.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
1084 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.8 to 0.93 |
| Manganese | Mn | 0.6 to 0.9 |
These are the limits of the standard's chemical range. High-carbon steel. Also known as: C86D (near), 1.1830 (near).
1084 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 715 °C (1319 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | Withheld | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 150 °C (303 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
1084 is hypereutectoid (carbon above about 0.8%), so it has no Ac3. The boundary that matters is Acm, where carbides dissolve, and the steel is normally hardened from between Ac1 and Acm.
Above about 0.8% carbon, normal hardening leaves some carbon locked in carbides. Less carbon is dissolved than the bulk analysis says, so the real Ms of 1084 sits higher than this estimate.
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 1084 steel at?
- Austenitize 1084 at 800 to 830 °C (1470 to 1525 °F), then quench: fast oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 1084 at?
- Temper 1084 at 175 to 230 °C (345 to 445 °F). Typical hardness: 57 to 60 HRC after a 190 to 200 C temper.
- What do you quench 1084 steel in?
- Fast oil. At eutectoid carbon everything transforms cleanly with no excess carbide to manage. Normalize after forging, then harden from a low soak. Pattern-welds beautifully against 15N20.
- What is 1084 steel equivalent to?
- Other designations for 1084, or for its nearest equivalent where marked "near": C86D (near), 1.1830 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other carbon steels
- 1018Low-carbon steel
- 1045Medium-carbon steel
- 1060Medium-high carbon steel
- 1075High-carbon steel
- 1080High-carbon steel
- 1095High-carbon steel
- 15N20Nickel band steel
- 26C3Very high carbon steel
Sources for this grade: SAE J403 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.