1018 vs 8620 steel
1018 (Low-carbon steel). The everyday mild steel. Too low in carbon to through-harden; case-harden it or use it as machined.
8620 (Case-hardening alloy steel). The standard carburizing steel for gears: glass-hard case over a tough low-carbon core.
How 1018 and 8620 differ
- Carbon is close: 0.15 to 0.2% in 1018 and 0.18 to 0.23% in 8620.
- 8620 is alloyed with nickel (0.4 to 0.7%) and chromium (0.4 to 0.6%), which 1018 does not have in any real amount.
- Both are austenitized in much the same range: 900 to 925 °C for 1018 and 900 to 925 °C for 8620.
- The quench differs. 1018: oil or water after carburizing. 8620: oil, direct or after reheating to about 815 to 845 C.
Side by side
| 1018 | 8620 | |
|---|---|---|
| Type | Low-carbon steel | Case-hardening alloy steel |
| Carbon (C), wt % | 0.15 to 0.2 | 0.18 to 0.23 |
| Manganese (Mn), wt % | 0.6 to 0.9 | 0.7 to 0.9 |
| Silicon (Si), wt % | none listed | 0.15 to 0.35 |
| Nickel (Ni), wt % | none listed | 0.4 to 0.7 |
| Chromium (Cr), wt % | none listed | 0.4 to 0.6 |
| Molybdenum (Mo), wt % | none listed | 0.15 to 0.25 |
| Austenitize | Carburize: 900 to 925 °C (1650 to 1695 °F) | Carburize: 900 to 925 °C (1650 to 1695 °F) |
| Quench | Oil or water after carburizing | Oil, direct or after reheating to about 815 to 845 C |
| Temper | 150 to 200 °C (300 to 390 °F) | 150 to 200 °C (300 to 390 °F) |
| Typical hardness | Case about 58 to 62 HRC, core stays soft | Case 58 to 62 HRC, core roughly 30 to 40 HRC |
| Ac1 (lower critical temperature) | about 715 °C (1319 °F) | about 721 °C (1330 °F) |
| Ac3 (upper critical temperature) | about 825 °C (1517 °F) | about 827 °C (1521 °F) |
| Ms (martensite start) | about 442 °C (828 °F) | about 411 °C (771 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
1018
Not a through-hardening steel. Gas or pack carburize to build a high-carbon case, quench, then temper low. As-supplied cold-drawn bar is often used with no heat treatment at all.
8620
Case depth is set by carburizing time and temperature, not by the quench. The alloy content keeps the core from collapsing under contact loads.
Questions
- What is the difference between 1018 and 8620 steel?
- Carbon is close: 0.15 to 0.2% in 1018 and 0.18 to 0.23% in 8620. 8620 is alloyed with nickel (0.4 to 0.7%) and chromium (0.4 to 0.6%), which 1018 does not have in any real amount.
- Is 1018 or 8620 harder after heat treatment?
- Typical hardness for 1018: case about 58 to 62 HRC, core stays soft. For 8620: case 58 to 62 HRC, core roughly 30 to 40 HRC. The result depends on the temper you choose.
- Can I heat treat 1018 and 8620 the same way?
- No, each has its own recipe. 1018: carburize at 900 to 925 °C, quench in oil or water after carburizing, temper at 150 to 200 °C. 8620: carburize at 900 to 925 °C, quench in oil, direct or after reheating to about 815 to 845 C, temper at 150 to 200 °C.
Heat treatment numbers for your own steel, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat