O1 vs D2 steel

O1 (Oil-hardening tool steel). The gauge-plate standard. Predictable, fine grained, and at home in every tool room and knife shop.

D2 (High-carbon high-chromium tool steel). The blanking-die classic: huge carbide volume, high wear resistance, semi-stainless behavior.

How O1 and D2 differ

  • D2 carries more carbon: 1.4 to 1.6% against 0.85 to 1% in O1.
  • O1 is alloyed with tungsten (0.4 to 0.6%), which D2 does not have in any real amount.
  • D2 is alloyed with molybdenum (0.7 to 1.2%) and vanadium (1.1 max%), which O1 does not have in any real amount.
  • D2 has far more chromium: 11 to 13% against 0.4 to 0.6%.
  • D2 is austenitized hotter: 1000 to 1030 °C (1830 to 1885 °F) against 790 to 815 °C (1455 to 1500 °F) for O1.
  • The quench differs. O1: oil. D2: air, plates, or vacuum gas quench.

Side by side

O1 and D2 compared
O1D2
TypeOil-hardening tool steelHigh-carbon high-chromium tool steel
Carbon (C), wt %0.85 to 11.4 to 1.6
Manganese (Mn), wt %1 to 1.40.6 max
Silicon (Si), wt %0.5 max0.6 max
Chromium (Cr), wt %0.4 to 0.611 to 13
Tungsten (W), wt %0.4 to 0.6none listed
Vanadium (V), wt %0.3 max1.1 max
Molybdenum (Mo), wt %none listed0.7 to 1.2
Austenitize790 to 815 °C (1455 to 1500 °F)1000 to 1030 °C (1830 to 1885 °F)
QuenchOilAir, plates, or vacuum gas quench
Temper150 to 260 °C (300 to 500 °F)200 to 530 °C (390 to 985 °F)
Typical hardness57 to 64 HRC depending on temper59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C
Ac1 (lower critical temperature)about 729 °C (1344 °F)Withheld
Ac3 (upper critical temperature)WithheldWithheld
Ms (martensite start)about 105 °C (221 °F)Withheld

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

O1

Soak 10 to 20 minutes at temperature. Moves little in the quench, which is why gauge makers standardized on it. Anneal at 760 to 790 C with a slow cool when you need to re-machine.

D2

Foil wrap and a proper soak of 30 to 45 minutes matter at these temperatures. Tempering near 520 C trades a little hardness for secondary carbides and is the route to take before coating. Cold treatment reduces retained austenite.

Questions

What is the difference between O1 and D2 steel?
D2 carries more carbon: 1.4 to 1.6% against 0.85 to 1% in O1. O1 is alloyed with tungsten (0.4 to 0.6%), which D2 does not have in any real amount.
Is O1 or D2 harder after heat treatment?
Typical hardness for O1: 57 to 64 HRC depending on temper. For D2: 59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C. The result depends on the temper you choose.
Can I heat treat O1 and D2 the same way?
No, each has its own recipe. O1: austenitize at 790 to 815 °C, quench in oil, temper at 150 to 260 °C. D2: austenitize at 1000 to 1030 °C, quench in air, plates, or vacuum gas quench, temper at 200 to 530 °C.