H13 steel heat treatment
The die-casting die steel: keeps its strength with the die at a red heat, cycle after cycle. Typical practice for H13: austenitize at 995 to 1040 °C (1825 to 1905 °F), quench (vacuum gas quench or still air), then temper at 550 to 620 °C (1020 to 1150 °F).
- Austenitize
- 995 to 1040 °C
- 1825 to 1905 °F
- Temper
- 550 to 620 °C
- 1020 to 1150 °F
- Quench
- Vacuum gas quench or still air
- Typical hardness
- 44 to 52 HRC after double or triple tempering
Always temper at least twice; the first temper transforms retained austenite that the second must then temper. Secondary hardening peaks near 510 to 550 C. Never leave it in the as-quenched state overnight.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
H13 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.32 to 0.45 |
| Manganese | Mn | 0.2 to 0.5 |
| Silicon | Si | 0.8 to 1.25 |
| Chromium | Cr | 4.75 to 5.5 |
| Molybdenum | Mo | 1.1 to 1.75 |
| Vanadium | V | 0.8 to 1.2 |
These are the limits of the standard's chemical range. Hot-work tool steel. Also known as: 1.2344, X40CrMoV5-1, SKD61.
H13 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | Withheld | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | Withheld | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | Withheld | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Chromium near 5.1% puts H13 outside the low-alloy steels these correlations were fitted to. High-chromium tool and stainless steels need measured data.
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden H13 steel at?
- Austenitize H13 at 995 to 1040 °C (1825 to 1905 °F), then quench: vacuum gas quench or still air. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper H13 at?
- Temper H13 at 550 to 620 °C (1020 to 1150 °F). Typical hardness: 44 to 52 HRC after double or triple tempering.
- What do you quench H13 steel in?
- Vacuum gas quench or still air. Always temper at least twice; the first temper transforms retained austenite that the second must then temper. Secondary hardening peaks near 510 to 550 C. Never leave it in the as-quenched state overnight.
- What is H13 steel equivalent to?
- Other designations for H13, or for its nearest equivalent where marked "near": 1.2344, X40CrMoV5-1, SKD61. Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other tool steels
- W1Water-hardening tool steel
- O1Oil-hardening tool steel
- A2Air-hardening tool steel
- D2High-carbon high-chromium tool steel
- S7Shock-resisting tool steel
- M2High-speed steel
Sources for this grade: ASTM A681 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat