The standard high-speed steel: drills and end mills that stay hard even glowing faint red. Typical practice for M2: austenitize at 1180 to 1220 °C (2155 to 2230 °F), quench (salt bath, oil, or vacuum gas quench), then temper at 540 to 570 °C (1005 to 1060 °F).
- Austenitize
- 1180 to 1220 °C
- 2155 to 2230 °F
- Temper
- 540 to 570 °C
- 1005 to 1060 °F
- Quench
- Salt bath, oil, or vacuum gas quench
- Typical hardness
- 63 to 66 HRC after triple tempering
Needs staged preheats on the way up and a triple temper on the way down; the hardness comes from secondary carbides, not the quench alone. Strictly a professional-furnace steel.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
M2 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.78 to 0.88 |
| Manganese | Mn | 0.15 to 0.4 |
| Silicon | Si | 0.2 to 0.45 |
| Chromium | Cr | 3.75 to 4.5 |
| Molybdenum | Mo | 4.5 to 5.5 |
| Tungsten | W | 5.5 to 6.75 |
| Vanadium | V | 1.75 to 2.2 |
These are the limits of the standard's chemical range. High-speed steel. Also known as: 1.3343, HS6-5-2C, SKH51.
M2 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | Withheld | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | Withheld | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | Withheld | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Chromium near 4.1% puts M2 outside the low-alloy steels these correlations were fitted to. High-chromium tool and stainless steels need measured data.
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden M2 steel at?
- Austenitize M2 at 1180 to 1220 °C (2155 to 2230 °F), then quench: salt bath, oil, or vacuum gas quench. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper M2 at?
- Temper M2 at 540 to 570 °C (1005 to 1060 °F). Typical hardness: 63 to 66 HRC after triple tempering.
- What do you quench M2 steel in?
- Salt bath, oil, or vacuum gas quench. Needs staged preheats on the way up and a triple temper on the way down; the hardness comes from secondary carbides, not the quench alone. Strictly a professional-furnace steel.
- What is M2 steel equivalent to?
- Other designations for M2, or for its nearest equivalent where marked "near": 1.3343, HS6-5-2C, SKH51. Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other tool steels
- W1Water-hardening tool steel
- O1Oil-hardening tool steel
- A2Air-hardening tool steel
- D2High-carbon high-chromium tool steel
- S7Shock-resisting tool steel
- H13Hot-work tool steel
Sources for this grade: ASTM A600 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat