O1 vs W1 steel
O1 (Oil-hardening tool steel). The gauge-plate standard. Predictable, fine grained, and at home in every tool room and knife shop.
W1 (Water-hardening tool steel). The old-school tool steel: plain high carbon, water quenched, hard skin over a tough core.
How O1 and W1 differ
- W1 carries more carbon: 0.95 to 1.1% against 0.85 to 1% in O1.
- O1 is alloyed with chromium (0.4 to 0.6%) and tungsten (0.4 to 0.6%), which W1 does not have in any real amount.
- O1 is austenitized hotter: 790 to 815 °C (1455 to 1500 °F) against 760 to 815 °C (1400 to 1500 °F) for W1.
- The quench differs. O1: oil. W1: water or brine, interrupted for thin sections.
Side by side
| O1 | W1 | |
|---|---|---|
| Type | Oil-hardening tool steel | Water-hardening tool steel |
| Carbon (C), wt % | 0.85 to 1 | 0.95 to 1.1 |
| Manganese (Mn), wt % | 1 to 1.4 | 0.25 |
| Silicon (Si), wt % | 0.5 max | 0.25 |
| Chromium (Cr), wt % | 0.4 to 0.6 | none listed |
| Tungsten (W), wt % | 0.4 to 0.6 | none listed |
| Vanadium (V), wt % | 0.3 max | none listed |
| Austenitize | 790 to 815 °C (1455 to 1500 °F) | 760 to 815 °C (1400 to 1500 °F) |
| Quench | Oil | Water or brine, interrupted for thin sections |
| Temper | 150 to 260 °C (300 to 500 °F) | 150 to 230 °C (300 to 445 °F) |
| Typical hardness | 57 to 64 HRC depending on temper | 58 to 64 HRC at the surface |
| Ac1 (lower critical temperature) | about 729 °C (1344 °F) | about 728 °C (1342 °F) |
| Ac3 (upper critical temperature) | Withheld | Withheld |
| Ms (martensite start) | about 105 °C (221 °F) | about 98 °C (208 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
O1
Soak 10 to 20 minutes at temperature. Moves little in the quench, which is why gauge makers standardized on it. Anneal at 760 to 790 C with a slow cool when you need to re-machine.
W1
The A681 specification spans carbon classes from 0.70 to 1.50; the values shown are a common cutlery class. Very shallow hardening, which is the feature: the core stays unhardened and tough.
Questions
- What is the difference between O1 and W1 steel?
- W1 carries more carbon: 0.95 to 1.1% against 0.85 to 1% in O1. O1 is alloyed with chromium (0.4 to 0.6%) and tungsten (0.4 to 0.6%), which W1 does not have in any real amount.
- Is O1 or W1 harder after heat treatment?
- Typical hardness for O1: 57 to 64 HRC depending on temper. For W1: 58 to 64 HRC at the surface. The result depends on the temper you choose.
- Can I heat treat O1 and W1 the same way?
- No, each has its own recipe. O1: austenitize at 790 to 815 °C, quench in oil, temper at 150 to 260 °C. W1: austenitize at 760 to 815 °C, quench in water or brine, interrupted for thin sections, temper at 150 to 230 °C.
Heat treatment numbers for your own steel, with sources.