Skip to content

4130 vs 4140 steel

4130 (Cr-Mo alloy steel). Chromoly. The weldable aircraft-tube and roll-cage steel, used normalized or quenched and tempered.

4140 (Cr-Mo alloy steel). The general-purpose quenched-and-tempered alloy steel: shafts, bolts, fixtures, tooling that must not snap.

How 4130 and 4140 differ

  • 4140 carries more carbon: 0.38 to 0.43% against 0.28 to 0.33% in 4130.
  • Both are austenitized in much the same range: 855 to 885 °C for 4130 and 845 to 870 °C for 4140.
  • The quench differs. 4130: oil, water for heavy sections. 4140: oil.

Side by side

4130 and 4140 compared
41304140
TypeCr-Mo alloy steelCr-Mo alloy steel
Carbon (C), wt %0.28 to 0.330.38 to 0.43
Manganese (Mn), wt %0.4 to 0.60.75 to 1
Silicon (Si), wt %0.15 to 0.350.15 to 0.35
Chromium (Cr), wt %0.8 to 1.10.8 to 1.1
Molybdenum (Mo), wt %0.15 to 0.250.15 to 0.25
Austenitize855 to 885 °C (1570 to 1625 °F)845 to 870 °C (1555 to 1600 °F)
QuenchOil, water for heavy sectionsOil
Temper400 to 565 °C (750 to 1050 °F)400 to 650 °C (750 to 1200 °F)
Typical hardness28 to 36 HRC quenched and temperedAbout 54 to 59 HRC as quenched, 28 to 36 HRC after machinery tempers
Ac1 (lower critical temperature)about 741 °C (1366 °F)about 737 °C (1359 °F)
Ac3 (upper critical temperature)about 815 °C (1500 °F)about 798 °C (1469 °F)
Ms (martensite start)about 382 °C (719 °F)about 328 °C (623 °F)

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

4130

The low carbon keeps welds tolerable, but thick or restrained joints still deserve preheat. Normalize at 870 to 925 C after welding when the design allows.

4140

Deep hardening and predictable. Many shops avoid tempering between about 260 and 370 C, where tempered martensite embrittlement costs toughness without buying hardness.

Questions

What is the difference between 4130 and 4140 steel?
4140 carries more carbon: 0.38 to 0.43% against 0.28 to 0.33% in 4130. Both are austenitized in much the same range: 855 to 885 °C for 4130 and 845 to 870 °C for 4140.
Is 4130 or 4140 harder after heat treatment?
Typical hardness for 4130: 28 to 36 HRC quenched and tempered. For 4140: about 54 to 59 HRC as quenched, 28 to 36 HRC after machinery tempers. The result depends on the temper you choose.
Can I heat treat 4130 and 4140 the same way?
No, each has its own recipe. 4130: austenitize at 855 to 885 °C, quench in oil, water for heavy sections, temper at 400 to 565 °C. 4140: austenitize at 845 to 870 °C, quench in oil, temper at 400 to 650 °C.

Heat treatment numbers for your own steel, with sources.

Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat

Get HeatTreat on Google Play