5160 vs 9260 steel
5160 (Cr spring steel). Leaf-spring steel and the sword maker's friend. Outstanding toughness with honest hardness.
9260 (Si-Mn spring steel). Silicon spring steel with legendary flex. A favorite for swords that must survive abuse.
How 5160 and 9260 differ
- Carbon is close: 0.56 to 0.64% in 5160 and 0.56 to 0.64% in 9260.
- 5160 is alloyed with chromium (0.7 to 0.9%), which 9260 does not have in any real amount.
- Both are austenitized in much the same range: 815 to 845 °C for 5160 and 815 to 870 °C for 9260.
- Both are quenched the same way: oil.
Side by side
| 5160 | 9260 | |
|---|---|---|
| Type | Cr spring steel | Si-Mn spring steel |
| Carbon (C), wt % | 0.56 to 0.64 | 0.56 to 0.64 |
| Manganese (Mn), wt % | 0.75 to 1 | 0.75 to 1 |
| Silicon (Si), wt % | 0.15 to 0.35 | 1.8 to 2.2 |
| Chromium (Cr), wt % | 0.7 to 0.9 | none listed |
| Austenitize | 815 to 845 °C (1500 to 1555 °F) | 815 to 870 °C (1500 to 1600 °F) |
| Quench | Oil | Oil |
| Temper | 190 to 480 °C (375 to 895 °F) | 190 to 480 °C (375 to 895 °F) |
| Typical hardness | 57 to 59 HRC at a 200 C temper for blades, 44 to 48 HRC at spring tempers | 57 to 59 HRC at a 200 C temper, 45 to 50 HRC at spring tempers |
| Ac1 (lower critical temperature) | about 734 °C (1354 °F) | about 772 °C (1421 °F) |
| Ac3 (upper critical temperature) | about 764 °C (1407 °F) | about 842 °C (1548 °F) |
| Ms (martensite start) | about 249 °C (480 °F) | about 259 °C (497 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
5160
The chromium buys hardenability, so ordinary oil works even on thick blades. For springs temper at 370 to 480 C.
9260
Silicon strengthens the ferrite and resists tempering, so it holds hardness at higher tempers than plain carbon steel. Decarburization in the forge is the thing to watch: silicon steels lose surface carbon quickly.
Questions
- What is the difference between 5160 and 9260 steel?
- Carbon is close: 0.56 to 0.64% in 5160 and 0.56 to 0.64% in 9260. 5160 is alloyed with chromium (0.7 to 0.9%), which 9260 does not have in any real amount.
- Is 5160 or 9260 harder after heat treatment?
- Typical hardness for 5160: 57 to 59 HRC at a 200 C temper for blades, 44 to 48 HRC at spring tempers. For 9260: 57 to 59 HRC at a 200 C temper, 45 to 50 HRC at spring tempers. The result depends on the temper you choose.
- Can I heat treat 5160 and 9260 the same way?
- No, each has its own recipe. 5160: austenitize at 815 to 845 °C, quench in oil, temper at 190 to 480 °C. 9260: austenitize at 815 to 870 °C, quench in oil, temper at 190 to 480 °C.
Heat treatment numbers for your own steel, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat