H13 vs S7 steel
H13 (Hot-work tool steel). The die-casting die steel: keeps its strength with the die at a red heat, cycle after cycle.
S7 (Shock-resisting tool steel). The jackhammer-bit steel: built to take impact at 54 to 57 HRC without shattering.
How H13 and S7 differ
- S7 carries more carbon: 0.45 to 0.55% against 0.32 to 0.45% in H13.
- H13 is alloyed with vanadium (0.8 to 1.2%), which S7 does not have in any real amount.
- H13 has far more chromium: 4.75 to 5.5% against 3 to 3.5%.
- H13 is austenitized hotter: 995 to 1040 °C (1825 to 1905 °F) against 925 to 955 °C (1695 to 1750 °F) for S7.
- The quench differs. H13: vacuum gas quench or still air. S7: air up to about 60 mm, otherwise interrupted oil.
Side by side
| H13 | S7 | |
|---|---|---|
| Type | Hot-work tool steel | Shock-resisting tool steel |
| Carbon (C), wt % | 0.32 to 0.45 | 0.45 to 0.55 |
| Manganese (Mn), wt % | 0.2 to 0.5 | 0.2 to 0.9 |
| Silicon (Si), wt % | 0.8 to 1.25 | 0.2 to 1 |
| Chromium (Cr), wt % | 4.75 to 5.5 | 3 to 3.5 |
| Molybdenum (Mo), wt % | 1.1 to 1.75 | 1.3 to 1.8 |
| Vanadium (V), wt % | 0.8 to 1.2 | none listed |
| Austenitize | 995 to 1040 °C (1825 to 1905 °F) | 925 to 955 °C (1695 to 1750 °F) |
| Quench | Vacuum gas quench or still air | Air up to about 60 mm, otherwise interrupted oil |
| Temper | 550 to 620 °C (1020 to 1150 °F) | 205 to 540 °C (400 to 1005 °F) |
| Typical hardness | 44 to 52 HRC after double or triple tempering | 54 to 57 HRC at a 205 C temper |
| Ac1 (lower critical temperature) | Withheld | about 790 °C (1453 °F) |
| Ac3 (upper critical temperature) | Withheld | about 842 °C (1548 °F) |
| Ms (martensite start) | Withheld | about 260 °C (500 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
H13
Always temper at least twice; the first temper transforms retained austenite that the second must then temper. Secondary hardening peaks near 510 to 550 C. Never leave it in the as-quenched state overnight.
S7
Air hardening in most sections, which keeps distortion down on chisels and punches. Temper immediately after the quench; shock steels resent waiting around untempered.
Questions
- What is the difference between H13 and S7 steel?
- S7 carries more carbon: 0.45 to 0.55% against 0.32 to 0.45% in H13. H13 is alloyed with vanadium (0.8 to 1.2%), which S7 does not have in any real amount.
- Is H13 or S7 harder after heat treatment?
- Typical hardness for H13: 44 to 52 HRC after double or triple tempering. For S7: 54 to 57 HRC at a 205 C temper. The result depends on the temper you choose.
- Can I heat treat H13 and S7 the same way?
- No, each has its own recipe. H13: austenitize at 995 to 1040 °C, quench in vacuum gas quench or still air, temper at 550 to 620 °C. S7: austenitize at 925 to 955 °C, quench in air up to about 60 mm, otherwise interrupted oil, temper at 205 to 540 °C.