9310 steel heat treatment
Aerospace gear steel: deep, tough, fatigue-resistant carburized cases on a very tough core. Typical practice for AISI 9310: carburize at 900 to 925 °C (1650 to 1695 °F), quench (oil), then temper at 150 to 200 °C (300 to 390 °F).
- Carburize
- 900 to 925 °C
- 1650 to 1695 °F
- Temper
- 150 to 200 °C
- 300 to 390 °F
- Quench
- Oil
- Typical hardness
- Case 58 to 62 HRC, core about 34 to 42 HRC
The high nickel makes the core exceptionally tough at low temperature. Used where a gear tooth failure is not an option.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
9310 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.08 to 0.13 |
| Manganese | Mn | 0.45 to 0.65 |
| Silicon | Si | 0.15 to 0.35 |
| Nickel | Ni | 3 to 3.5 |
| Chromium | Cr | 1 to 1.4 |
| Molybdenum | Mo | 0.08 to 0.15 |
These are the limits of the standard's chemical range. Case-hardening alloy steel. Also known as: 832M13 (near), 1.6657 (near).
9310 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 690 °C (1274 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 810 °C (1489 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 405 °C (761 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you carburize 9310 steel at?
- Carburize 9310 at 900 to 925 °C (1650 to 1695 °F), then quench: oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 9310 at?
- Temper 9310 at 150 to 200 °C (300 to 390 °F). Typical hardness: case 58 to 62 HRC, core about 34 to 42 HRC.
- What do you quench 9310 steel in?
- Oil. The high nickel makes the core exceptionally tough at low temperature. Used where a gear tooth failure is not an option.
- What is 9310 steel equivalent to?
- Other designations for 9310, or for its nearest equivalent where marked "near": 832M13 (near), 1.6657 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other alloy steels
- 4130Cr-Mo alloy steel
- 4140Cr-Mo alloy steel
- 4340Ni-Cr-Mo alloy steel
- 5160Cr spring steel
- 6150Cr-V spring steel
- 8620Case-hardening alloy steel
- 9260Si-Mn spring steel
- 52100Bearing steel
- 80CrV2Cr-V high carbon steel
- 300MUltra-high-strength steel
Sources for this grade: SAE J404 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat