1080 vs 1084 steel
1080 (High-carbon steel). Near-eutectoid carbon steel: simple, predictable, and hard to get badly wrong.
1084 (High-carbon steel). The classic beginner blade steel: eutectoid carbon, wide forgiving windows, clean results in a home shop.
How 1080 and 1084 differ
- 1084 carries more carbon: 0.8 to 0.93% against 0.75 to 0.88% in 1080.
- Both are austenitized in much the same range: 800 to 830 °C for 1080 and 800 to 830 °C for 1084.
- Both are quenched the same way: fast oil.
Side by side
| 1080 | 1084 | |
|---|---|---|
| Type | High-carbon steel | High-carbon steel |
| Carbon (C), wt % | 0.75 to 0.88 | 0.8 to 0.93 |
| Manganese (Mn), wt % | 0.6 to 0.9 | 0.6 to 0.9 |
| Austenitize | 800 to 830 °C (1470 to 1525 °F) | 800 to 830 °C (1470 to 1525 °F) |
| Quench | Fast oil | Fast oil |
| Temper | 175 to 260 °C (345 to 500 °F) | 175 to 230 °C (345 to 445 °F) |
| Typical hardness | 56 to 59 HRC after a 200 C temper | 57 to 60 HRC after a 190 to 200 C temper |
| Ac1 (lower critical temperature) | about 715 °C (1319 °F) | about 715 °C (1319 °F) |
| Ac3 (upper critical temperature) | Withheld | Withheld |
| Ms (martensite start) | about 171 °C (341 °F) | about 150 °C (303 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
1080
Being close to the eutectoid, it needs no long soak: heat through, hold briefly, quench. Excellent first forging steel.
1084
At eutectoid carbon everything transforms cleanly with no excess carbide to manage. Normalize after forging, then harden from a low soak. Pattern-welds beautifully against 15N20.
Questions
- What is the difference between 1080 and 1084 steel?
- 1084 carries more carbon: 0.8 to 0.93% against 0.75 to 0.88% in 1080. Both are austenitized in much the same range: 800 to 830 °C for 1080 and 800 to 830 °C for 1084.
- Is 1080 or 1084 harder after heat treatment?
- Typical hardness for 1080: 56 to 59 HRC after a 200 C temper. For 1084: 57 to 60 HRC after a 190 to 200 C temper. The result depends on the temper you choose.
- Can I heat treat 1080 and 1084 the same way?
- No, each has its own recipe. 1080: austenitize at 800 to 830 °C, quench in fast oil, temper at 175 to 260 °C. 1084: austenitize at 800 to 830 °C, quench in fast oil, temper at 175 to 230 °C.
Heat treatment numbers for your own steel, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat