1018 vs 1045 steel
1018 (Low-carbon steel). The everyday mild steel. Too low in carbon to through-harden; case-harden it or use it as machined.
1045 (Medium-carbon steel). The workhorse medium-carbon steel for shafts, axles and machine parts, used quenched and tempered.
How 1018 and 1045 differ
- 1045 carries more carbon: 0.43 to 0.5% against 0.15 to 0.2% in 1018.
- 1018 is austenitized hotter: 900 to 925 °C (1650 to 1695 °F) against 815 to 845 °C (1500 to 1555 °F) for 1045.
- The quench differs. 1018: oil or water after carburizing. 1045: water or brine, oil for thin sections.
Side by side
| 1018 | 1045 | |
|---|---|---|
| Type | Low-carbon steel | Medium-carbon steel |
| Carbon (C), wt % | 0.15 to 0.2 | 0.43 to 0.5 |
| Manganese (Mn), wt % | 0.6 to 0.9 | 0.6 to 0.9 |
| Austenitize | Carburize: 900 to 925 °C (1650 to 1695 °F) | 815 to 845 °C (1500 to 1555 °F) |
| Quench | Oil or water after carburizing | Water or brine, oil for thin sections |
| Temper | 150 to 200 °C (300 to 390 °F) | 315 to 595 °C (600 to 1105 °F) |
| Typical hardness | Case about 58 to 62 HRC, core stays soft | About 55 HRC as quenched at the surface, 20 to 30 HRC after machinery tempers |
| Ac1 (lower critical temperature) | about 715 °C (1319 °F) | about 715 °C (1319 °F) |
| Ac3 (upper critical temperature) | about 825 °C (1517 °F) | about 772 °C (1421 °F) |
| Ms (martensite start) | about 442 °C (828 °F) | about 320 °C (607 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
1018
Not a through-hardening steel. Gas or pack carburize to build a high-carbon case, quench, then temper low. As-supplied cold-drawn bar is often used with no heat treatment at all.
1045
Shallow hardening: heavy sections harden at the skin only. Water quenching risks distortion and cracks on sharp corners, so radius and pre-machine generously.
Questions
- What is the difference between 1018 and 1045 steel?
- 1045 carries more carbon: 0.43 to 0.5% against 0.15 to 0.2% in 1018. 1018 is austenitized hotter: 900 to 925 °C (1650 to 1695 °F) against 815 to 845 °C (1500 to 1555 °F) for 1045.
- Is 1018 or 1045 harder after heat treatment?
- Typical hardness for 1018: case about 58 to 62 HRC, core stays soft. For 1045: about 55 HRC as quenched at the surface, 20 to 30 HRC after machinery tempers. The result depends on the temper you choose.
- Can I heat treat 1018 and 1045 the same way?
- No, each has its own recipe. 1018: carburize at 900 to 925 °C, quench in oil or water after carburizing, temper at 150 to 200 °C. 1045: austenitize at 815 to 845 °C, quench in water or brine, oil for thin sections, temper at 315 to 595 °C.