D2 steel heat treatment
The blanking-die classic: huge carbide volume, high wear resistance, semi-stainless behavior. Typical practice for D2: austenitize at 1000 to 1030 °C (1830 to 1885 °F), quench (air, plates, or vacuum gas quench), then temper at 200 to 530 °C (390 to 985 °F).
- Austenitize
- 1000 to 1030 °C
- 1830 to 1885 °F
- Temper
- 200 to 530 °C
- 390 to 985 °F
- Quench
- Air, plates, or vacuum gas quench
- Typical hardness
- 59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C
Foil wrap and a proper soak of 30 to 45 minutes matter at these temperatures. Tempering near 520 C trades a little hardness for secondary carbides and is the route to take before coating. Cold treatment reduces retained austenite.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
D2 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 1.4 to 1.6 |
| Manganese | Mn | 0.6 max |
| Silicon | Si | 0.6 max |
| Chromium | Cr | 11 to 13 |
| Molybdenum | Mo | 0.7 to 1.2 |
| Vanadium | V | 1.1 max |
These are the limits of the standard's chemical range. High-carbon high-chromium tool steel. Also known as: 1.2379, X153CrMoV12, SKD11.
D2 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | Withheld | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | Withheld | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | Withheld | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Carbon near 1.50% is beyond the range these correlations were fitted to.
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden D2 steel at?
- Austenitize D2 at 1000 to 1030 °C (1830 to 1885 °F), then quench: air, plates, or vacuum gas quench. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper D2 at?
- Temper D2 at 200 to 530 °C (390 to 985 °F). Typical hardness: 59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C.
- What do you quench D2 steel in?
- Air, plates, or vacuum gas quench. Foil wrap and a proper soak of 30 to 45 minutes matter at these temperatures. Tempering near 520 C trades a little hardness for secondary carbides and is the route to take before coating. Cold treatment reduces retained austenite.
- What is D2 steel equivalent to?
- Other designations for D2, or for its nearest equivalent where marked "near": 1.2379, X153CrMoV12, SKD11. Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other tool steels
- W1Water-hardening tool steel
- O1Oil-hardening tool steel
- A2Air-hardening tool steel
- S7Shock-resisting tool steel
- H13Hot-work tool steel
- M2High-speed steel
Sources for this grade: ASTM A681 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat