1095 steel heat treatment

The traditional razor and knife steel. Hard, keen, and demanding about its quench. Typical practice for AISI 1095: austenitize at 790 to 815 °C (1455 to 1500 °F), quench (very fast oil), then temper at 175 to 230 °C (345 to 445 °F).

Austenitize
790 to 815 °C
1455 to 1500 °F
Temper
175 to 230 °C
345 to 445 °F
Quench
Very fast oil
Typical hardness
58 to 62 HRC after a 190 C temper

Hypereutectoid and low in manganese, so it is shallow hardening and wants a genuinely fast oil. Keep the soak short at the low end of the range so excess carbide stays undissolved and grain stays fine. Brine hardens it deeper but cracks are a real risk.

Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

1095 chemical composition

1095 chemical composition in weight per cent
ElementSymbolWeight %
CarbonC0.9 to 1.03
ManganeseMn0.3 to 0.5

These are the limits of the standard's chemical range. High-carbon steel. Also known as: C100 (near), 1.1274 (near), SK95 (near).

1095 critical temperatures

Estimated critical temperatures for 1095
TemperatureWhat it meansEstimateEquation
Ac1Lower critical temperatureabout 719 °C (1326 °F)Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W
Ac3Upper critical temperatureWithheldAc3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W
MsMartensite startabout 119 °C (246 °F)Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo

1095 is hypereutectoid (carbon above about 0.8%), so it has no Ac3. The boundary that matters is Acm, where carbides dissolve, and the steel is normally hardened from between Ac1 and Acm.

Above about 0.8% carbon, normal hardening leaves some carbon locked in carbides. Less carbon is dissolved than the bulk analysis says, so the real Ms of 1095 sits higher than this estimate.

Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.

Questions

What temperature do you harden 1095 steel at?
Austenitize 1095 at 790 to 815 °C (1455 to 1500 °F), then quench: very fast oil. This is typical published practice; section size and furnace accuracy shift the right number.
What temperature do you temper 1095 at?
Temper 1095 at 175 to 230 °C (345 to 445 °F). Typical hardness: 58 to 62 HRC after a 190 C temper.
What do you quench 1095 steel in?
Very fast oil. Hypereutectoid and low in manganese, so it is shallow hardening and wants a genuinely fast oil. Keep the soak short at the low end of the range so excess carbide stays undissolved and grain stays fine. Brine hardens it deeper but cracks are a real risk.
What is 1095 steel equivalent to?
Other designations for 1095, or for its nearest equivalent where marked "near": C100 (near), 1.1274 (near), SK95 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.

Enter your own composition and get the numbers, with sources.

Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat

Get HeatTreat on Google Play