5160 vs 80CrV2 steel
5160 (Cr spring steel). Leaf-spring steel and the sword maker's friend. Outstanding toughness with honest hardness.
80CrV2 (Cr-V high carbon steel). European chopper steel: 1080 with a little chromium and vanadium for deeper hardening and finer grain.
How 5160 and 80CrV2 differ
- 80CrV2 carries more carbon: 0.75 to 0.85% against 0.56 to 0.64% in 5160.
- Both are austenitized in much the same range: 815 to 845 °C for 5160 and 800 to 840 °C for 80CrV2.
- The quench differs. 5160: oil. 80CrV2: fast oil.
Side by side
| 5160 | 80CrV2 | |
|---|---|---|
| Type | Cr spring steel | Cr-V high carbon steel |
| Carbon (C), wt % | 0.56 to 0.64 | 0.75 to 0.85 |
| Manganese (Mn), wt % | 0.75 to 1 | 0.3 to 0.5 |
| Silicon (Si), wt % | 0.15 to 0.35 | 0.15 to 0.35 |
| Chromium (Cr), wt % | 0.7 to 0.9 | 0.4 to 0.6 |
| Vanadium (V), wt % | none listed | 0.15 to 0.25 |
| Austenitize | 815 to 845 °C (1500 to 1555 °F) | 800 to 840 °C (1470 to 1545 °F) |
| Quench | Oil | Fast oil |
| Temper | 190 to 480 °C (375 to 895 °F) | 175 to 230 °C (345 to 445 °F) |
| Typical hardness | 57 to 59 HRC at a 200 C temper for blades, 44 to 48 HRC at spring tempers | 56 to 60 HRC after a 200 C temper |
| Ac1 (lower critical temperature) | about 734 °C (1354 °F) | about 734 °C (1354 °F) |
| Ac3 (upper critical temperature) | about 764 °C (1407 °F) | about 760 °C (1401 °F) |
| Ms (martensite start) | about 249 °C (480 °F) | about 182 °C (360 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
5160
The chromium buys hardenability, so ordinary oil works even on thick blades. For springs temper at 370 to 480 C.
80CrV2
Handles thicker blades than plain 1080 thanks to the chromium. The vanadium keeps grain fine even with forge heats that wander hot.
Questions
- What is the difference between 5160 and 80CrV2 steel?
- 80CrV2 carries more carbon: 0.75 to 0.85% against 0.56 to 0.64% in 5160. Both are austenitized in much the same range: 815 to 845 °C for 5160 and 800 to 840 °C for 80CrV2.
- Is 5160 or 80CrV2 harder after heat treatment?
- Typical hardness for 5160: 57 to 59 HRC at a 200 C temper for blades, 44 to 48 HRC at spring tempers. For 80CrV2: 56 to 60 HRC after a 200 C temper. The result depends on the temper you choose.
- Can I heat treat 5160 and 80CrV2 the same way?
- No, each has its own recipe. 5160: austenitize at 815 to 845 °C, quench in oil, temper at 190 to 480 °C. 80CrV2: austenitize at 800 to 840 °C, quench in fast oil, temper at 175 to 230 °C.
Heat treatment numbers for your own steel, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat