Skip to content

8620 vs 9310 steel

8620 (Case-hardening alloy steel). The standard carburizing steel for gears: glass-hard case over a tough low-carbon core.

9310 (Case-hardening alloy steel). Aerospace gear steel: deep, tough, fatigue-resistant carburized cases on a very tough core.

How 8620 and 9310 differ

  • 8620 carries more carbon: 0.18 to 0.23% against 0.08 to 0.13% in 9310.
  • Both are austenitized in much the same range: 900 to 925 °C for 8620 and 900 to 925 °C for 9310.
  • The quench differs. 8620: oil, direct or after reheating to about 815 to 845 C. 9310: oil.

Side by side

8620 and 9310 compared
86209310
TypeCase-hardening alloy steelCase-hardening alloy steel
Carbon (C), wt %0.18 to 0.230.08 to 0.13
Manganese (Mn), wt %0.7 to 0.90.45 to 0.65
Silicon (Si), wt %0.15 to 0.350.15 to 0.35
Nickel (Ni), wt %0.4 to 0.73 to 3.5
Chromium (Cr), wt %0.4 to 0.61 to 1.4
Molybdenum (Mo), wt %0.15 to 0.250.08 to 0.15
AustenitizeCarburize: 900 to 925 °C (1650 to 1695 °F)Carburize: 900 to 925 °C (1650 to 1695 °F)
QuenchOil, direct or after reheating to about 815 to 845 COil
Temper150 to 200 °C (300 to 390 °F)150 to 200 °C (300 to 390 °F)
Typical hardnessCase 58 to 62 HRC, core roughly 30 to 40 HRCCase 58 to 62 HRC, core about 34 to 42 HRC
Ac1 (lower critical temperature)about 721 °C (1330 °F)about 690 °C (1274 °F)
Ac3 (upper critical temperature)about 827 °C (1521 °F)about 810 °C (1489 °F)
Ms (martensite start)about 411 °C (771 °F)about 405 °C (761 °F)

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

8620

Case depth is set by carburizing time and temperature, not by the quench. The alloy content keeps the core from collapsing under contact loads.

9310

The high nickel makes the core exceptionally tough at low temperature. Used where a gear tooth failure is not an option.

Questions

What is the difference between 8620 and 9310 steel?
8620 carries more carbon: 0.18 to 0.23% against 0.08 to 0.13% in 9310. Both are austenitized in much the same range: 900 to 925 °C for 8620 and 900 to 925 °C for 9310.
Is 8620 or 9310 harder after heat treatment?
Typical hardness for 8620: case 58 to 62 HRC, core roughly 30 to 40 HRC. For 9310: case 58 to 62 HRC, core about 34 to 42 HRC. The result depends on the temper you choose.
Can I heat treat 8620 and 9310 the same way?
No, each has its own recipe. 8620: carburize at 900 to 925 °C, quench in oil, direct or after reheating to about 815 to 845 C, temper at 150 to 200 °C. 9310: carburize at 900 to 925 °C, quench in oil, temper at 150 to 200 °C.

Heat treatment numbers for your own steel, with sources.

Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat

Get HeatTreat on Google Play