Skip to content

1095 vs 26C3 steel

1095 (High-carbon steel). The traditional razor and knife steel. Hard, keen, and demanding about its quench.

26C3 (Very high carbon steel). Very high purity, very high carbon razor steel. Extremely keen edges and vivid hamons in skilled hands.

How 1095 and 26C3 differ

  • 26C3 carries more carbon: 1.25% against 0.9 to 1.03% in 1095.
  • Both are austenitized in much the same range: 790 to 815 °C for 1095 and 790 to 815 °C for 26C3.
  • The quench differs. 1095: very fast oil. 26C3: fast oil, brine only on thin blades by experienced hands.

Side by side

1095 and 26C3 compared
109526C3
TypeHigh-carbon steelVery high carbon steel
Carbon (C), wt %0.9 to 1.031.25
Manganese (Mn), wt %0.3 to 0.50.35
Silicon (Si), wt %none listed0.25
Austenitize790 to 815 °C (1455 to 1500 °F)790 to 815 °C (1455 to 1500 °F)
QuenchVery fast oilFast oil, brine only on thin blades by experienced hands
Temper175 to 230 °C (345 to 445 °F)150 to 200 °C (300 to 390 °F)
Typical hardness58 to 62 HRC after a 190 C temper62 to 65 HRC after a low temper
Ac1 (lower critical temperature)about 719 °C (1326 °F)Withheld
Ac3 (upper critical temperature)WithheldWithheld
Ms (martensite start)about 119 °C (246 °F)Withheld

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

1095

Hypereutectoid and low in manganese, so it is shallow hardening and wants a genuinely fast oil. Keep the soak short at the low end of the range so excess carbide stays undissolved and grain stays fine. Brine hardens it deeper but cracks are a real risk.

26C3

Keep soaks short and temperatures low so the large carbon reserve stays mostly in carbide. Shallow hardening: thick spines stay soft and hamons come easily.

Questions

What is the difference between 1095 and 26C3 steel?
26C3 carries more carbon: 1.25% against 0.9 to 1.03% in 1095. Both are austenitized in much the same range: 790 to 815 °C for 1095 and 790 to 815 °C for 26C3.
Is 1095 or 26C3 harder after heat treatment?
Typical hardness for 1095: 58 to 62 HRC after a 190 C temper. For 26C3: 62 to 65 HRC after a low temper. The result depends on the temper you choose.
Can I heat treat 1095 and 26C3 the same way?
No, each has its own recipe. 1095: austenitize at 790 to 815 °C, quench in very fast oil, temper at 175 to 230 °C. 26C3: austenitize at 790 to 815 °C, quench in fast oil, brine only on thin blades by experienced hands, temper at 150 to 200 °C.

Heat treatment numbers for your own steel, with sources.

Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat

Get HeatTreat on Google Play