1084 vs 15N20 steel
1084 (High-carbon steel). The classic beginner blade steel: eutectoid carbon, wide forgiving windows, clean results in a home shop.
15N20 (Nickel band steel). Band-saw steel and the bright layer in pattern-welded damascus. Tough, fine grained, resists etching dark.
How 1084 and 15N20 differ
- 1084 carries more carbon: 0.8 to 0.93% against 0.75% in 15N20.
- 15N20 is alloyed with nickel (2%), which 1084 does not have in any real amount.
- Both are austenitized in much the same range: 800 to 830 °C for 1084 and 790 to 815 °C for 15N20.
- Both are quenched the same way: fast oil.
Side by side
| 1084 | 15N20 | |
|---|---|---|
| Type | High-carbon steel | Nickel band steel |
| Carbon (C), wt % | 0.8 to 0.93 | 0.75 |
| Manganese (Mn), wt % | 0.6 to 0.9 | 0.4 |
| Nickel (Ni), wt % | none listed | 2 |
| Austenitize | 800 to 830 °C (1470 to 1525 °F) | 790 to 815 °C (1455 to 1500 °F) |
| Quench | Fast oil | Fast oil |
| Temper | 175 to 230 °C (345 to 445 °F) | 175 to 230 °C (345 to 445 °F) |
| Typical hardness | 57 to 60 HRC after a 190 to 200 C temper | 57 to 60 HRC after a 200 C temper |
| Ac1 (lower critical temperature) | about 715 °C (1319 °F) | about 685 °C (1265 °F) |
| Ac3 (upper critical temperature) | Withheld | about 704 °C (1299 °F) |
| Ms (martensite start) | about 150 °C (303 °F) | about 174 °C (346 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
1084
At eutectoid carbon everything transforms cleanly with no excess carbide to manage. Normalize after forging, then harden from a low soak. Pattern-welds beautifully against 15N20.
15N20
Heat treats almost identically to 1084, which is exactly why the two make an easy damascus pair. The nickel stays bright in ferric chloride etch.
Questions
- What is the difference between 1084 and 15N20 steel?
- 1084 carries more carbon: 0.8 to 0.93% against 0.75% in 15N20. 15N20 is alloyed with nickel (2%), which 1084 does not have in any real amount.
- Is 1084 or 15N20 harder after heat treatment?
- Typical hardness for 1084: 57 to 60 HRC after a 190 to 200 C temper. For 15N20: 57 to 60 HRC after a 200 C temper. The result depends on the temper you choose.
- Can I heat treat 1084 and 15N20 the same way?
- No, each has its own recipe. 1084: austenitize at 800 to 830 °C, quench in fast oil, temper at 175 to 230 °C. 15N20: austenitize at 790 to 815 °C, quench in fast oil, temper at 175 to 230 °C.