A2 vs D2 steel
A2 (Air-hardening tool steel). Air-hardening die steel: the stability of a gas quench with real wear resistance. A fine hard-use knife steel.
D2 (High-carbon high-chromium tool steel). The blanking-die classic: huge carbide volume, high wear resistance, semi-stainless behavior.
How A2 and D2 differ
- D2 carries more carbon: 1.4 to 1.6% against 0.95 to 1.05% in A2.
- D2 has far more chromium: 11 to 13% against 4.75 to 5.5%.
- D2 is austenitized hotter: 1000 to 1030 °C (1830 to 1885 °F) against 925 to 980 °C (1695 to 1795 °F) for A2.
- The quench differs. A2: still air or aluminium plates. D2: air, plates, or vacuum gas quench.
Side by side
| A2 | D2 | |
|---|---|---|
| Type | Air-hardening tool steel | High-carbon high-chromium tool steel |
| Carbon (C), wt % | 0.95 to 1.05 | 1.4 to 1.6 |
| Manganese (Mn), wt % | 1 max | 0.6 max |
| Silicon (Si), wt % | 0.5 max | 0.6 max |
| Chromium (Cr), wt % | 4.75 to 5.5 | 11 to 13 |
| Molybdenum (Mo), wt % | 0.9 to 1.4 | 0.7 to 1.2 |
| Vanadium (V), wt % | 0.15 to 0.5 | 1.1 max |
| Austenitize | 925 to 980 °C (1695 to 1795 °F) | 1000 to 1030 °C (1830 to 1885 °F) |
| Quench | Still air or aluminium plates | Air, plates, or vacuum gas quench |
| Temper | 175 to 230 °C (345 to 445 °F) | 200 to 530 °C (390 to 985 °F) |
| Typical hardness | 57 to 62 HRC | 59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C |
| Ac1 (lower critical temperature) | Withheld | Withheld |
| Ac3 (upper critical temperature) | Withheld | Withheld |
| Ms (martensite start) | Withheld | Withheld |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
A2
Wrap in stainless foil against decarburization, soak 20 to 45 minutes, cool in still air. Double tempering is standard practice. Distortion is low enough to harden finished parts.
D2
Foil wrap and a proper soak of 30 to 45 minutes matter at these temperatures. Tempering near 520 C trades a little hardness for secondary carbides and is the route to take before coating. Cold treatment reduces retained austenite.
Questions
- What is the difference between A2 and D2 steel?
- D2 carries more carbon: 1.4 to 1.6% against 0.95 to 1.05% in A2. D2 has far more chromium: 11 to 13% against 4.75 to 5.5%.
- Is A2 or D2 harder after heat treatment?
- Typical hardness for A2: 57 to 62 HRC. For D2: 59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C. The result depends on the temper you choose.
- Can I heat treat A2 and D2 the same way?
- No, each has its own recipe. A2: austenitize at 925 to 980 °C, quench in still air or aluminium plates, temper at 175 to 230 °C. D2: austenitize at 1000 to 1030 °C, quench in air, plates, or vacuum gas quench, temper at 200 to 530 °C.
Heat treatment numbers for your own steel, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat