440C steel heat treatment
The classic high-hardness stainless for bearings, valve seats and knives that must not rust. Typical practice for 440C: austenitize at 1010 to 1065 °C (1850 to 1950 °F), quench (air, plates, or oil), then temper at 150 to 230 °C (300 to 445 °F).
- Austenitize
- 1010 to 1065 °C
- 1850 to 1950 °F
- Temper
- 150 to 230 °C
- 300 to 445 °F
- Quench
- Air, plates, or oil
- Typical hardness
- 57 to 60 HRC
Cold treatment after the quench is common to convert retained austenite. Avoid tempering between about 425 and 565 C, where corrosion resistance and toughness both fall.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
440C chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.95 to 1.2 |
| Manganese | Mn | 1 max |
| Silicon | Si | 1 max |
| Chromium | Cr | 16 to 18 |
| Molybdenum | Mo | 0.75 max |
These are the limits of the standard's chemical range. Martensitic stainless steel. Also known as: 1.4125, X105CrMo17, SUS440C.
440C critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | Withheld | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | Withheld | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | Withheld | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Chromium near 17.0% puts 440C outside the low-alloy steels these correlations were fitted to. High-chromium tool and stainless steels need measured data.
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 440C steel at?
- Austenitize 440C at 1010 to 1065 °C (1850 to 1950 °F), then quench: air, plates, or oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 440C at?
- Temper 440C at 150 to 230 °C (300 to 445 °F). Typical hardness: 57 to 60 HRC.
- What do you quench 440C steel in?
- Air, plates, or oil. Cold treatment after the quench is common to convert retained austenite. Avoid tempering between about 425 and 565 C, where corrosion resistance and toughness both fall.
- What is 440C steel equivalent to?
- Other designations for 440C, or for its nearest equivalent where marked "near": 1.4125, X105CrMo17, SUS440C. Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other stainless steels
- 420Martensitic stainless steel
- AEB-LMartensitic stainless steel
- 154CMMartensitic stainless steel
- MagnaCutPowder-metallurgy stainless steel
Sources for this grade: ASTM A276 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat