4140 vs 8620 steel
4140 (Cr-Mo alloy steel). The general-purpose quenched-and-tempered alloy steel: shafts, bolts, fixtures, tooling that must not snap.
8620 (Case-hardening alloy steel). The standard carburizing steel for gears: glass-hard case over a tough low-carbon core.
How 4140 and 8620 differ
- 4140 carries more carbon: 0.38 to 0.43% against 0.18 to 0.23% in 8620.
- 8620 is alloyed with nickel (0.4 to 0.7%), which 4140 does not have in any real amount.
- 8620 is austenitized hotter: 900 to 925 °C (1650 to 1695 °F) against 845 to 870 °C (1555 to 1600 °F) for 4140.
- The quench differs. 4140: oil. 8620: oil, direct or after reheating to about 815 to 845 C.
Side by side
| 4140 | 8620 | |
|---|---|---|
| Type | Cr-Mo alloy steel | Case-hardening alloy steel |
| Carbon (C), wt % | 0.38 to 0.43 | 0.18 to 0.23 |
| Manganese (Mn), wt % | 0.75 to 1 | 0.7 to 0.9 |
| Silicon (Si), wt % | 0.15 to 0.35 | 0.15 to 0.35 |
| Chromium (Cr), wt % | 0.8 to 1.1 | 0.4 to 0.6 |
| Molybdenum (Mo), wt % | 0.15 to 0.25 | 0.15 to 0.25 |
| Nickel (Ni), wt % | none listed | 0.4 to 0.7 |
| Austenitize | 845 to 870 °C (1555 to 1600 °F) | Carburize: 900 to 925 °C (1650 to 1695 °F) |
| Quench | Oil | Oil, direct or after reheating to about 815 to 845 C |
| Temper | 400 to 650 °C (750 to 1200 °F) | 150 to 200 °C (300 to 390 °F) |
| Typical hardness | About 54 to 59 HRC as quenched, 28 to 36 HRC after machinery tempers | Case 58 to 62 HRC, core roughly 30 to 40 HRC |
| Ac1 (lower critical temperature) | about 737 °C (1359 °F) | about 721 °C (1330 °F) |
| Ac3 (upper critical temperature) | about 798 °C (1469 °F) | about 827 °C (1521 °F) |
| Ms (martensite start) | about 328 °C (623 °F) | about 411 °C (771 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
4140
Deep hardening and predictable. Many shops avoid tempering between about 260 and 370 C, where tempered martensite embrittlement costs toughness without buying hardness.
8620
Case depth is set by carburizing time and temperature, not by the quench. The alloy content keeps the core from collapsing under contact loads.
Questions
- What is the difference between 4140 and 8620 steel?
- 4140 carries more carbon: 0.38 to 0.43% against 0.18 to 0.23% in 8620. 8620 is alloyed with nickel (0.4 to 0.7%), which 4140 does not have in any real amount.
- Is 4140 or 8620 harder after heat treatment?
- Typical hardness for 4140: about 54 to 59 HRC as quenched, 28 to 36 HRC after machinery tempers. For 8620: case 58 to 62 HRC, core roughly 30 to 40 HRC. The result depends on the temper you choose.
- Can I heat treat 4140 and 8620 the same way?
- No, each has its own recipe. 4140: austenitize at 845 to 870 °C, quench in oil, temper at 400 to 650 °C. 8620: carburize at 900 to 925 °C, quench in oil, direct or after reheating to about 815 to 845 C, temper at 150 to 200 °C.
Heat treatment numbers for your own steel, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat