Skip to content

O1 steel heat treatment

The gauge-plate standard. Predictable, fine grained, and at home in every tool room and knife shop. Typical practice for O1: austenitize at 790 to 815 °C (1455 to 1500 °F), quench (oil), then temper at 150 to 260 °C (300 to 500 °F).

Austenitize
790 to 815 °C
1455 to 1500 °F
Temper
150 to 260 °C
300 to 500 °F
Quench
Oil
Typical hardness
57 to 64 HRC depending on temper

Soak 10 to 20 minutes at temperature. Moves little in the quench, which is why gauge makers standardized on it. Anneal at 760 to 790 C with a slow cool when you need to re-machine.

Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

O1 chemical composition

O1 chemical composition in weight per cent
ElementSymbolWeight %
CarbonC0.85 to 1
ManganeseMn1 to 1.4
SiliconSi0.5 max
ChromiumCr0.4 to 0.6
TungstenW0.4 to 0.6
VanadiumV0.3 max

These are the limits of the standard's chemical range. Oil-hardening tool steel. Also known as: 1.2510, 100MnCrW4, SKS3 (near).

O1 critical temperatures

Estimated critical temperatures for O1
TemperatureWhat it meansEstimateEquation
Ac1Lower critical temperatureabout 729 °C (1344 °F)Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W
Ac3Upper critical temperatureWithheldAc3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W
MsMartensite startabout 105 °C (221 °F)Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo

O1 is hypereutectoid (carbon above about 0.8%), so it has no Ac3. The boundary that matters is Acm, where carbides dissolve, and the steel is normally hardened from between Ac1 and Acm.

Above about 0.8% carbon, normal hardening leaves some carbon locked in carbides. Less carbon is dissolved than the bulk analysis says, so the real Ms of O1 sits higher than this estimate.

Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.

Questions

What temperature do you harden O1 steel at?
Austenitize O1 at 790 to 815 °C (1455 to 1500 °F), then quench: oil. This is typical published practice; section size and furnace accuracy shift the right number.
What temperature do you temper O1 at?
Temper O1 at 150 to 260 °C (300 to 500 °F). Typical hardness: 57 to 64 HRC depending on temper.
What do you quench O1 steel in?
Oil. Soak 10 to 20 minutes at temperature. Moves little in the quench, which is why gauge makers standardized on it. Anneal at 760 to 790 C with a slow cool when you need to re-machine.
What is O1 steel equivalent to?
Other designations for O1, or for its nearest equivalent where marked "near": 1.2510, 100MnCrW4, SKS3 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.

Enter your own composition and get the numbers, with sources.

Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat

Get HeatTreat on Google Play