300M steel heat treatment
Landing-gear steel: 4340 with added silicon and vanadium, run at very high strength. Typical practice for 300M: austenitize at 855 to 885 °C (1570 to 1625 °F), quench (oil), then temper at 285 to 315 °C (545 to 600 °F).
- Austenitize
- 855 to 885 °C
- 1570 to 1625 °F
- Temper
- 285 to 315 °C
- 545 to 600 °F
- Quench
- Oil
- Typical hardness
- 52 to 55 HRC, tensile strength around 1900 to 2000 MPa
The silicon pushes tempered martensite embrittlement above the working temper, which is what lets it run at a 300 C temper safely. Double temper. Aerospace use demands vacuum-melt quality and hydrogen control.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
300M chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.4 to 0.46 |
| Manganese | Mn | 0.65 to 0.9 |
| Silicon | Si | 1.45 to 1.8 |
| Nickel | Ni | 1.65 to 2 |
| Chromium | Cr | 0.7 to 0.95 |
| Molybdenum | Mo | 0.3 to 0.45 |
| Vanadium | V | 0.05 to 0.1 |
These are the limits of the standard's chemical range. Ultra-high-strength steel. Also known as: 4340M, S155 (spec).
300M critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 745 °C (1373 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 841 °C (1547 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 288 °C (551 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 300M steel at?
- Austenitize 300M at 855 to 885 °C (1570 to 1625 °F), then quench: oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 300M at?
- Temper 300M at 285 to 315 °C (545 to 600 °F). Typical hardness: 52 to 55 HRC, tensile strength around 1900 to 2000 MPa.
- What do you quench 300M steel in?
- Oil. The silicon pushes tempered martensite embrittlement above the working temper, which is what lets it run at a 300 C temper safely. Double temper. Aerospace use demands vacuum-melt quality and hydrogen control.
- What is 300M steel equivalent to?
- Other designations for 300M, or for its nearest equivalent where marked "near": 4340M, S155 (spec). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other alloy steels
- 4130Cr-Mo alloy steel
- 4140Cr-Mo alloy steel
- 4340Ni-Cr-Mo alloy steel
- 5160Cr spring steel
- 6150Cr-V spring steel
- 8620Case-hardening alloy steel
- 9260Si-Mn spring steel
- 9310Case-hardening alloy steel
- 52100Bearing steel
- 80CrV2Cr-V high carbon steel
Sources for this grade: AMS 6257 and producer datasheets; Typical published practice.