1095 (High-carbon steel). The traditional razor and knife steel. Hard, keen, and demanding about its quench.

O1 (Oil-hardening tool steel). The gauge-plate standard. Predictable, fine grained, and at home in every tool room and knife shop.

How 1095 and O1 differ

  • Carbon is close: 0.9 to 1.03% in 1095 and 0.85 to 1% in O1.
  • O1 is alloyed with chromium (0.4 to 0.6%) and tungsten (0.4 to 0.6%), which 1095 does not have in any real amount.
  • Both are austenitized in much the same range: 790 to 815 °C for 1095 and 790 to 815 °C for O1.
  • The quench differs. 1095: very fast oil. O1: oil.

Side by side

1095 and O1 compared
1095O1
TypeHigh-carbon steelOil-hardening tool steel
Carbon (C), wt %0.9 to 1.030.85 to 1
Manganese (Mn), wt %0.3 to 0.51 to 1.4
Silicon (Si), wt %none listed0.5 max
Chromium (Cr), wt %none listed0.4 to 0.6
Tungsten (W), wt %none listed0.4 to 0.6
Vanadium (V), wt %none listed0.3 max
Austenitize790 to 815 °C (1455 to 1500 °F)790 to 815 °C (1455 to 1500 °F)
QuenchVery fast oilOil
Temper175 to 230 °C (345 to 445 °F)150 to 260 °C (300 to 500 °F)
Typical hardness58 to 62 HRC after a 190 C temper57 to 64 HRC depending on temper
Ac1 (lower critical temperature)about 719 °C (1326 °F)about 729 °C (1344 °F)
Ac3 (upper critical temperature)WithheldWithheld
Ms (martensite start)about 119 °C (246 °F)about 105 °C (221 °F)

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

1095

Hypereutectoid and low in manganese, so it is shallow hardening and wants a genuinely fast oil. Keep the soak short at the low end of the range so excess carbide stays undissolved and grain stays fine. Brine hardens it deeper but cracks are a real risk.

O1

Soak 10 to 20 minutes at temperature. Moves little in the quench, which is why gauge makers standardized on it. Anneal at 760 to 790 C with a slow cool when you need to re-machine.

Questions

What is the difference between 1095 and O1 steel?
Carbon is close: 0.9 to 1.03% in 1095 and 0.85 to 1% in O1. O1 is alloyed with chromium (0.4 to 0.6%) and tungsten (0.4 to 0.6%), which 1095 does not have in any real amount.
Is 1095 or O1 harder after heat treatment?
Typical hardness for 1095: 58 to 62 HRC after a 190 C temper. For O1: 57 to 64 HRC depending on temper. The result depends on the temper you choose.
Can I heat treat 1095 and O1 the same way?
No, each has its own recipe. 1095: austenitize at 790 to 815 °C, quench in very fast oil, temper at 175 to 230 °C. O1: austenitize at 790 to 815 °C, quench in oil, temper at 150 to 260 °C.

Heat treatment numbers for your own steel, with sources.