300M vs 4340 steel

300M (Ultra-high-strength steel). Landing-gear steel: 4340 with added silicon and vanadium, run at very high strength.

4340 (Ni-Cr-Mo alloy steel). The deep-hardening high-strength steel for crankshafts, gears and aircraft parts. Strong and tough at once.

How 300M and 4340 differ

  • Carbon is close: 0.4 to 0.46% in 300M and 0.38 to 0.43% in 4340.
  • 300M is alloyed with molybdenum (0.3 to 0.45%), which 4340 does not have in any real amount.
  • 300M is austenitized hotter: 855 to 885 °C (1570 to 1625 °F) against 815 to 845 °C (1500 to 1555 °F) for 4340.
  • Both are quenched the same way: oil.

Side by side

300M and 4340 compared
300M4340
TypeUltra-high-strength steelNi-Cr-Mo alloy steel
Carbon (C), wt %0.4 to 0.460.38 to 0.43
Manganese (Mn), wt %0.65 to 0.90.6 to 0.8
Silicon (Si), wt %1.45 to 1.80.15 to 0.35
Nickel (Ni), wt %1.65 to 21.65 to 2
Chromium (Cr), wt %0.7 to 0.950.7 to 0.9
Molybdenum (Mo), wt %0.3 to 0.450.2 to 0.3
Vanadium (V), wt %0.05 to 0.1none listed
Austenitize855 to 885 °C (1570 to 1625 °F)815 to 845 °C (1500 to 1555 °F)
QuenchOilOil
Temper285 to 315 °C (545 to 600 °F)200 to 650 °C (390 to 1200 °F)
Typical hardness52 to 55 HRC, tensile strength around 1900 to 2000 MPaAbout 53 to 55 HRC as quenched, chosen temper sets the strength class
Ac1 (lower critical temperature)about 745 °C (1373 °F)about 705 °C (1302 °F)
Ac3 (upper critical temperature)about 841 °C (1547 °F)about 772 °C (1422 °F)
Ms (martensite start)about 288 °C (551 °F)about 303 °C (577 °F)

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

300M

The silicon pushes tempered martensite embrittlement above the working temper, which is what lets it run at a 300 C temper safely. Double temper. Aerospace use demands vacuum-melt quality and hydrogen control.

4340

Hardens through in large sections thanks to nickel plus chromium plus molybdenum. Avoid tempering in the embrittlement window around 260 to 370 C.

Questions

What is the difference between 300M and 4340 steel?
Carbon is close: 0.4 to 0.46% in 300M and 0.38 to 0.43% in 4340. 300M is alloyed with molybdenum (0.3 to 0.45%), which 4340 does not have in any real amount.
Is 300M or 4340 harder after heat treatment?
Typical hardness for 300M: 52 to 55 HRC, tensile strength around 1900 to 2000 MPa. For 4340: about 53 to 55 HRC as quenched, chosen temper sets the strength class. The result depends on the temper you choose.
Can I heat treat 300M and 4340 the same way?
No, each has its own recipe. 300M: austenitize at 855 to 885 °C, quench in oil, temper at 285 to 315 °C. 4340: austenitize at 815 to 845 °C, quench in oil, temper at 200 to 650 °C.