1045 steel heat treatment
The workhorse medium-carbon steel for shafts, axles and machine parts, used quenched and tempered. Typical practice for AISI 1045: austenitize at 815 to 845 °C (1500 to 1555 °F), quench (water or brine, oil for thin sections), then temper at 315 to 595 °C (600 to 1105 °F).
- Austenitize
- 815 to 845 °C
- 1500 to 1555 °F
- Temper
- 315 to 595 °C
- 600 to 1105 °F
- Quench
- Water or brine, oil for thin sections
- Typical hardness
- About 55 HRC as quenched at the surface, 20 to 30 HRC after machinery tempers
Shallow hardening: heavy sections harden at the skin only. Water quenching risks distortion and cracks on sharp corners, so radius and pre-machine generously.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
1045 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.43 to 0.5 |
| Manganese | Mn | 0.6 to 0.9 |
These are the limits of the standard's chemical range. Medium-carbon steel. Also known as: C45, 1.0503, S45C, En8 (near), 080M40 (near).
1045 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 715 °C (1319 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 772 °C (1421 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 320 °C (607 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 1045 steel at?
- Austenitize 1045 at 815 to 845 °C (1500 to 1555 °F), then quench: water or brine, oil for thin sections. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 1045 at?
- Temper 1045 at 315 to 595 °C (600 to 1105 °F). Typical hardness: about 55 HRC as quenched at the surface, 20 to 30 HRC after machinery tempers.
- What do you quench 1045 steel in?
- Water or brine, oil for thin sections. Shallow hardening: heavy sections harden at the skin only. Water quenching risks distortion and cracks on sharp corners, so radius and pre-machine generously.
- What is 1045 steel equivalent to?
- Other designations for 1045, or for its nearest equivalent where marked "near": C45, 1.0503, S45C, En8 (near), 080M40 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other carbon steels
- 1018Low-carbon steel
- 1060Medium-high carbon steel
- 1075High-carbon steel
- 1080High-carbon steel
- 1084High-carbon steel
- 1095High-carbon steel
- 15N20Nickel band steel
- 26C3Very high carbon steel
Sources for this grade: SAE J403 chemical ranges; Typical published practice.