Skip to content

A2 steel heat treatment

Air-hardening die steel: the stability of a gas quench with real wear resistance. A fine hard-use knife steel. Typical practice for A2: austenitize at 925 to 980 °C (1695 to 1795 °F), quench (still air or aluminium plates), then temper at 175 to 230 °C (345 to 445 °F).

Austenitize
925 to 980 °C
1695 to 1795 °F
Temper
175 to 230 °C
345 to 445 °F
Quench
Still air or aluminium plates
Typical hardness
57 to 62 HRC

Wrap in stainless foil against decarburization, soak 20 to 45 minutes, cool in still air. Double tempering is standard practice. Distortion is low enough to harden finished parts.

Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

A2 chemical composition

A2 chemical composition in weight per cent
ElementSymbolWeight %
CarbonC0.95 to 1.05
ManganeseMn1 max
SiliconSi0.5 max
ChromiumCr4.75 to 5.5
MolybdenumMo0.9 to 1.4
VanadiumV0.15 to 0.5

These are the limits of the standard's chemical range. Air-hardening tool steel. Also known as: 1.2363, X100CrMoV5, SKD12.

A2 critical temperatures

Estimated critical temperatures for A2
TemperatureWhat it meansEstimateEquation
Ac1Lower critical temperatureWithheldAc1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W
Ac3Upper critical temperatureWithheldAc3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W
MsMartensite startWithheldMs = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo

Chromium near 5.1% puts A2 outside the low-alloy steels these correlations were fitted to. High-chromium tool and stainless steels need measured data.

Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.

Questions

What temperature do you harden A2 steel at?
Austenitize A2 at 925 to 980 °C (1695 to 1795 °F), then quench: still air or aluminium plates. This is typical published practice; section size and furnace accuracy shift the right number.
What temperature do you temper A2 at?
Temper A2 at 175 to 230 °C (345 to 445 °F). Typical hardness: 57 to 62 HRC.
What do you quench A2 steel in?
Still air or aluminium plates. Wrap in stainless foil against decarburization, soak 20 to 45 minutes, cool in still air. Double tempering is standard practice. Distortion is low enough to harden finished parts.
What is A2 steel equivalent to?
Other designations for A2, or for its nearest equivalent where marked "near": 1.2363, X100CrMoV5, SKD12. Check the chemistry on your supplier's datasheet before treating them as the same steel.

Enter your own composition and get the numbers, with sources.

Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat

Get HeatTreat on Google Play