Skip to content

5160 steel heat treatment

Leaf-spring steel and the sword maker's friend. Outstanding toughness with honest hardness. Typical practice for AISI 5160: austenitize at 815 to 845 °C (1500 to 1555 °F), quench (oil), then temper at 190 to 480 °C (375 to 895 °F).

Austenitize
815 to 845 °C
1500 to 1555 °F
Temper
190 to 480 °C
375 to 895 °F
Quench
Oil
Typical hardness
57 to 59 HRC at a 200 C temper for blades, 44 to 48 HRC at spring tempers

The chromium buys hardenability, so ordinary oil works even on thick blades. For springs temper at 370 to 480 C.

Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

5160 chemical composition

5160 chemical composition in weight per cent
ElementSymbolWeight %
CarbonC0.56 to 0.64
ManganeseMn0.75 to 1
SiliconSi0.15 to 0.35
ChromiumCr0.7 to 0.9

These are the limits of the standard's chemical range. Cr spring steel. Also known as: 55Cr3 (near), 1.7176 (near), 527A60 (near).

5160 critical temperatures

Estimated critical temperatures for 5160
TemperatureWhat it meansEstimateEquation
Ac1Lower critical temperatureabout 734 °C (1354 °F)Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W
Ac3Upper critical temperatureabout 764 °C (1407 °F)Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W
MsMartensite startabout 249 °C (480 °F)Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo

Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.

Questions

What temperature do you harden 5160 steel at?
Austenitize 5160 at 815 to 845 °C (1500 to 1555 °F), then quench: oil. This is typical published practice; section size and furnace accuracy shift the right number.
What temperature do you temper 5160 at?
Temper 5160 at 190 to 480 °C (375 to 895 °F). Typical hardness: 57 to 59 HRC at a 200 C temper for blades, 44 to 48 HRC at spring tempers.
What do you quench 5160 steel in?
Oil. The chromium buys hardenability, so ordinary oil works even on thick blades. For springs temper at 370 to 480 C.
What is 5160 steel equivalent to?
Other designations for 5160, or for its nearest equivalent where marked "near": 55Cr3 (near), 1.7176 (near), 527A60 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.

Enter your own composition and get the numbers, with sources.

Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat