440C vs AEB-L steel
440C (Martensitic stainless steel). The classic high-hardness stainless for bearings, valve seats and knives that must not rust.
AEB-L (Martensitic stainless steel). Razor-blade stainless: fine carbides, high hardness, and shocking toughness for the price.
How 440C and AEB-L differ
- 440C carries more carbon: 0.95 to 1.2% against 0.67% in AEB-L.
- 440C is alloyed with molybdenum (0.75 max%), which AEB-L does not have in any real amount.
- 440C has far more chromium: 16 to 18% against 12.8%.
- AEB-L is austenitized hotter: 1050 to 1080 °C (1920 to 1975 °F) against 1010 to 1065 °C (1850 to 1950 °F) for 440C.
- The quench differs. 440C: air, plates, or oil. AEB-L: aluminium plates with forced air, then cold treatment.
Side by side
| 440C | AEB-L | |
|---|---|---|
| Type | Martensitic stainless steel | Martensitic stainless steel |
| Carbon (C), wt % | 0.95 to 1.2 | 0.67 |
| Manganese (Mn), wt % | 1 max | 0.6 |
| Silicon (Si), wt % | 1 max | 0.4 |
| Chromium (Cr), wt % | 16 to 18 | 12.8 |
| Molybdenum (Mo), wt % | 0.75 max | none listed |
| Austenitize | 1010 to 1065 °C (1850 to 1950 °F) | 1050 to 1080 °C (1920 to 1975 °F) |
| Quench | Air, plates, or oil | Aluminium plates with forced air, then cold treatment |
| Temper | 150 to 230 °C (300 to 445 °F) | 150 to 200 °C (300 to 390 °F) |
| Typical hardness | 57 to 60 HRC | 60 to 63 HRC with cold treatment |
| Ac1 (lower critical temperature) | Withheld | Withheld |
| Ac3 (upper critical temperature) | Withheld | Withheld |
| Ms (martensite start) | Withheld | Withheld |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
440C
Cold treatment after the quench is common to convert retained austenite. Avoid tempering between about 425 and 565 C, where corrosion resistance and toughness both fall.
AEB-L
The composition is balanced so nearly all carbide dissolves, so soak times are short, about 10 to 15 minutes, and the cold treatment genuinely matters for reaching full hardness.
Questions
- What is the difference between 440C and AEB-L steel?
- 440C carries more carbon: 0.95 to 1.2% against 0.67% in AEB-L. 440C is alloyed with molybdenum (0.75 max%), which AEB-L does not have in any real amount.
- Is 440C or AEB-L harder after heat treatment?
- Typical hardness for 440C: 57 to 60 HRC. For AEB-L: 60 to 63 HRC with cold treatment. The result depends on the temper you choose.
- Can I heat treat 440C and AEB-L the same way?
- No, each has its own recipe. 440C: austenitize at 1010 to 1065 °C, quench in air, plates, or oil, temper at 150 to 230 °C. AEB-L: austenitize at 1050 to 1080 °C, quench in aluminium plates with forced air, then cold treatment, temper at 150 to 200 °C.
Heat treatment numbers for your own steel, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat