52100 steel heat treatment
Ball-bearing steel, and one of the finest fine-edge knife steels when heat treated with care. Typical practice for AISI 52100: austenitize at 840 to 860 °C (1545 to 1580 °F), quench (oil), then temper at 160 to 230 °C (320 to 445 °F).
- Austenitize
- 840 to 860 °C
- 1545 to 1580 °F
- Temper
- 160 to 230 °C
- 320 to 445 °F
- Quench
- Oil
- Typical hardness
- 58 to 64 HRC depending on temper
Harden from the spheroidized condition with a modest soak of 10 to 20 minutes. Hypereutectoid, so the right austenitizing dissolves only part of the carbide. Cold treatment can cut retained austenite when maximum stability matters.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
52100 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.98 to 1.1 |
| Manganese | Mn | 0.25 to 0.45 |
| Silicon | Si | 0.15 to 0.35 |
| Chromium | Cr | 1.3 to 1.6 |
These are the limits of the standard's chemical range. Bearing steel. Also known as: 100Cr6, 1.3505, En31, 535A99, SUJ2, GCr15.
52100 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 751 °C (1384 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | Withheld | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 71 °C (160 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
52100 is hypereutectoid (carbon above about 0.8%), so it has no Ac3. The boundary that matters is Acm, where carbides dissolve, and the steel is normally hardened from between Ac1 and Acm.
Above about 0.8% carbon, normal hardening leaves some carbon locked in carbides. Less carbon is dissolved than the bulk analysis says, so the real Ms of 52100 sits higher than this estimate.
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 52100 steel at?
- Austenitize 52100 at 840 to 860 °C (1545 to 1580 °F), then quench: oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 52100 at?
- Temper 52100 at 160 to 230 °C (320 to 445 °F). Typical hardness: 58 to 64 HRC depending on temper.
- What do you quench 52100 steel in?
- Oil. Harden from the spheroidized condition with a modest soak of 10 to 20 minutes. Hypereutectoid, so the right austenitizing dissolves only part of the carbide. Cold treatment can cut retained austenite when maximum stability matters.
- What is 52100 steel equivalent to?
- Other designations for 52100, or for its nearest equivalent where marked "near": 100Cr6, 1.3505, En31, 535A99, SUJ2, GCr15. Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other alloy steels
- 4130Cr-Mo alloy steel
- 4140Cr-Mo alloy steel
- 4340Ni-Cr-Mo alloy steel
- 5160Cr spring steel
- 6150Cr-V spring steel
- 8620Case-hardening alloy steel
- 9260Si-Mn spring steel
- 9310Case-hardening alloy steel
- 80CrV2Cr-V high carbon steel
- 300MUltra-high-strength steel
Sources for this grade: SAE J404 and ASTM A295 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.