52100 vs O1 steel
52100 (Bearing steel). Ball-bearing steel, and one of the finest fine-edge knife steels when heat treated with care.
O1 (Oil-hardening tool steel). The gauge-plate standard. Predictable, fine grained, and at home in every tool room and knife shop.
How 52100 and O1 differ
- 52100 carries more carbon: 0.98 to 1.1% against 0.85 to 1% in O1.
- O1 is alloyed with tungsten (0.4 to 0.6%), which 52100 does not have in any real amount.
- 52100 is austenitized hotter: 840 to 860 °C (1545 to 1580 °F) against 790 to 815 °C (1455 to 1500 °F) for O1.
- Both are quenched the same way: oil.
Side by side
| 52100 | O1 | |
|---|---|---|
| Type | Bearing steel | Oil-hardening tool steel |
| Carbon (C), wt % | 0.98 to 1.1 | 0.85 to 1 |
| Manganese (Mn), wt % | 0.25 to 0.45 | 1 to 1.4 |
| Silicon (Si), wt % | 0.15 to 0.35 | 0.5 max |
| Chromium (Cr), wt % | 1.3 to 1.6 | 0.4 to 0.6 |
| Tungsten (W), wt % | none listed | 0.4 to 0.6 |
| Vanadium (V), wt % | none listed | 0.3 max |
| Austenitize | 840 to 860 °C (1545 to 1580 °F) | 790 to 815 °C (1455 to 1500 °F) |
| Quench | Oil | Oil |
| Temper | 160 to 230 °C (320 to 445 °F) | 150 to 260 °C (300 to 500 °F) |
| Typical hardness | 58 to 64 HRC depending on temper | 57 to 64 HRC depending on temper |
| Ac1 (lower critical temperature) | about 751 °C (1384 °F) | about 729 °C (1344 °F) |
| Ac3 (upper critical temperature) | Withheld | Withheld |
| Ms (martensite start) | about 71 °C (160 °F) | about 105 °C (221 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
52100
Harden from the spheroidized condition with a modest soak of 10 to 20 minutes. Hypereutectoid, so the right austenitizing dissolves only part of the carbide. Cold treatment can cut retained austenite when maximum stability matters.
O1
Soak 10 to 20 minutes at temperature. Moves little in the quench, which is why gauge makers standardized on it. Anneal at 760 to 790 C with a slow cool when you need to re-machine.
Questions
- What is the difference between 52100 and O1 steel?
- 52100 carries more carbon: 0.98 to 1.1% against 0.85 to 1% in O1. O1 is alloyed with tungsten (0.4 to 0.6%), which 52100 does not have in any real amount.
- Is 52100 or O1 harder after heat treatment?
- Typical hardness for 52100: 58 to 64 HRC depending on temper. For O1: 57 to 64 HRC depending on temper. The result depends on the temper you choose.
- Can I heat treat 52100 and O1 the same way?
- No, each has its own recipe. 52100: austenitize at 840 to 860 °C, quench in oil, temper at 160 to 230 °C. O1: austenitize at 790 to 815 °C, quench in oil, temper at 150 to 260 °C.
Heat treatment numbers for your own steel, with sources.