4140 (Cr-Mo alloy steel). The general-purpose quenched-and-tempered alloy steel: shafts, bolts, fixtures, tooling that must not snap.

4340 (Ni-Cr-Mo alloy steel). The deep-hardening high-strength steel for crankshafts, gears and aircraft parts. Strong and tough at once.

How 4140 and 4340 differ

  • Carbon is close: 0.38 to 0.43% in 4140 and 0.38 to 0.43% in 4340.
  • 4340 is alloyed with nickel (1.65 to 2%), which 4140 does not have in any real amount.
  • 4140 is austenitized hotter: 845 to 870 °C (1555 to 1600 °F) against 815 to 845 °C (1500 to 1555 °F) for 4340.
  • Both are quenched the same way: oil.

Side by side

4140 and 4340 compared
41404340
TypeCr-Mo alloy steelNi-Cr-Mo alloy steel
Carbon (C), wt %0.38 to 0.430.38 to 0.43
Manganese (Mn), wt %0.75 to 10.6 to 0.8
Silicon (Si), wt %0.15 to 0.350.15 to 0.35
Chromium (Cr), wt %0.8 to 1.10.7 to 0.9
Molybdenum (Mo), wt %0.15 to 0.250.2 to 0.3
Nickel (Ni), wt %none listed1.65 to 2
Austenitize845 to 870 °C (1555 to 1600 °F)815 to 845 °C (1500 to 1555 °F)
QuenchOilOil
Temper400 to 650 °C (750 to 1200 °F)200 to 650 °C (390 to 1200 °F)
Typical hardnessAbout 54 to 59 HRC as quenched, 28 to 36 HRC after machinery tempersAbout 53 to 55 HRC as quenched, chosen temper sets the strength class
Ac1 (lower critical temperature)about 737 °C (1359 °F)about 705 °C (1302 °F)
Ac3 (upper critical temperature)about 798 °C (1469 °F)about 772 °C (1422 °F)
Ms (martensite start)about 328 °C (623 °F)about 303 °C (577 °F)

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

4140

Deep hardening and predictable. Many shops avoid tempering between about 260 and 370 C, where tempered martensite embrittlement costs toughness without buying hardness.

4340

Hardens through in large sections thanks to nickel plus chromium plus molybdenum. Avoid tempering in the embrittlement window around 260 to 370 C.

Questions

What is the difference between 4140 and 4340 steel?
Carbon is close: 0.38 to 0.43% in 4140 and 0.38 to 0.43% in 4340. 4340 is alloyed with nickel (1.65 to 2%), which 4140 does not have in any real amount.
Is 4140 or 4340 harder after heat treatment?
Typical hardness for 4140: about 54 to 59 HRC as quenched, 28 to 36 HRC after machinery tempers. For 4340: about 53 to 55 HRC as quenched, chosen temper sets the strength class. The result depends on the temper you choose.
Can I heat treat 4140 and 4340 the same way?
No, each has its own recipe. 4140: austenitize at 845 to 870 °C, quench in oil, temper at 400 to 650 °C. 4340: austenitize at 815 to 845 °C, quench in oil, temper at 200 to 650 °C.