1060 steel heat treatment
A tough sword and spring carbon steel. Takes a good edge yet bends before it breaks. Typical practice for AISI 1060: austenitize at 800 to 830 °C (1470 to 1525 °F), quench (medium-fast oil), then temper at 175 to 370 °C (345 to 700 °F).
- Austenitize
- 800 to 830 °C
- 1470 to 1525 °F
- Temper
- 175 to 370 °C
- 345 to 700 °F
- Quench
- Medium-fast oil
- Typical hardness
- 56 to 58 HRC with a 200 C temper, lower for springs
A favorite for large blades because the lower carbon leaves more ductility than 1084 or 1095 at the same temper.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
1060 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.55 to 0.65 |
| Manganese | Mn | 0.6 to 0.9 |
These are the limits of the standard's chemical range. Medium-high carbon steel. Also known as: C60 (near), S58C (near).
1060 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 715 °C (1319 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 753 °C (1387 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 262 °C (504 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 1060 steel at?
- Austenitize 1060 at 800 to 830 °C (1470 to 1525 °F), then quench: medium-fast oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 1060 at?
- Temper 1060 at 175 to 370 °C (345 to 700 °F). Typical hardness: 56 to 58 HRC with a 200 C temper, lower for springs.
- What do you quench 1060 steel in?
- Medium-fast oil. A favorite for large blades because the lower carbon leaves more ductility than 1084 or 1095 at the same temper.
- What is 1060 steel equivalent to?
- Other designations for 1060, or for its nearest equivalent where marked "near": C60 (near), S58C (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other carbon steels
- 1018Low-carbon steel
- 1045Medium-carbon steel
- 1075High-carbon steel
- 1080High-carbon steel
- 1084High-carbon steel
- 1095High-carbon steel
- 15N20Nickel band steel
- 26C3Very high carbon steel
Sources for this grade: SAE J403 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.