4140 steel heat treatment
The general-purpose quenched-and-tempered alloy steel: shafts, bolts, fixtures, tooling that must not snap. Typical practice for AISI 4140: austenitize at 845 to 870 °C (1555 to 1600 °F), quench (oil), then temper at 400 to 650 °C (750 to 1200 °F).
- Austenitize
- 845 to 870 °C
- 1555 to 1600 °F
- Temper
- 400 to 650 °C
- 750 to 1200 °F
- Quench
- Oil
- Typical hardness
- About 54 to 59 HRC as quenched, 28 to 36 HRC after machinery tempers
Deep hardening and predictable. Many shops avoid tempering between about 260 and 370 C, where tempered martensite embrittlement costs toughness without buying hardness.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
4140 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.38 to 0.43 |
| Manganese | Mn | 0.75 to 1 |
| Silicon | Si | 0.15 to 0.35 |
| Chromium | Cr | 0.8 to 1.1 |
| Molybdenum | Mo | 0.15 to 0.25 |
These are the limits of the standard's chemical range. Cr-Mo alloy steel. Also known as: 42CrMo4, 1.7225, En19, 708M40, SCM440.
4140 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 737 °C (1359 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 798 °C (1469 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 328 °C (623 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 4140 steel at?
- Austenitize 4140 at 845 to 870 °C (1555 to 1600 °F), then quench: oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 4140 at?
- Temper 4140 at 400 to 650 °C (750 to 1200 °F). Typical hardness: about 54 to 59 HRC as quenched, 28 to 36 HRC after machinery tempers.
- What do you quench 4140 steel in?
- Oil. Deep hardening and predictable. Many shops avoid tempering between about 260 and 370 C, where tempered martensite embrittlement costs toughness without buying hardness.
- What is 4140 steel equivalent to?
- Other designations for 4140, or for its nearest equivalent where marked "near": 42CrMo4, 1.7225, En19, 708M40, SCM440. Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other alloy steels
- 4130Cr-Mo alloy steel
- 4340Ni-Cr-Mo alloy steel
- 5160Cr spring steel
- 6150Cr-V spring steel
- 8620Case-hardening alloy steel
- 9260Si-Mn spring steel
- 9310Case-hardening alloy steel
- 52100Bearing steel
- 80CrV2Cr-V high carbon steel
- 300MUltra-high-strength steel
Sources for this grade: SAE J404 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat