Skip to content

D2 vs M2 steel

D2 (High-carbon high-chromium tool steel). The blanking-die classic: huge carbide volume, high wear resistance, semi-stainless behavior.

M2 (High-speed steel). The standard high-speed steel: drills and end mills that stay hard even glowing faint red.

How D2 and M2 differ

  • D2 carries more carbon: 1.4 to 1.6% against 0.78 to 0.88% in M2.
  • M2 is alloyed with tungsten (5.5 to 6.75%), which D2 does not have in any real amount.
  • D2 has far more chromium: 11 to 13% against 3.75 to 4.5%.
  • M2 is austenitized hotter: 1180 to 1220 °C (2155 to 2230 °F) against 1000 to 1030 °C (1830 to 1885 °F) for D2.
  • The quench differs. D2: air, plates, or vacuum gas quench. M2: salt bath, oil, or vacuum gas quench.

Side by side

D2 and M2 compared
D2M2
TypeHigh-carbon high-chromium tool steelHigh-speed steel
Carbon (C), wt %1.4 to 1.60.78 to 0.88
Manganese (Mn), wt %0.6 max0.15 to 0.4
Silicon (Si), wt %0.6 max0.2 to 0.45
Chromium (Cr), wt %11 to 133.75 to 4.5
Molybdenum (Mo), wt %0.7 to 1.24.5 to 5.5
Vanadium (V), wt %1.1 max1.75 to 2.2
Tungsten (W), wt %none listed5.5 to 6.75
Austenitize1000 to 1030 °C (1830 to 1885 °F)1180 to 1220 °C (2155 to 2230 °F)
QuenchAir, plates, or vacuum gas quenchSalt bath, oil, or vacuum gas quench
Temper200 to 530 °C (390 to 985 °F)540 to 570 °C (1005 to 1060 °F)
Typical hardness59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C63 to 66 HRC after triple tempering
Ac1 (lower critical temperature)WithheldWithheld
Ac3 (upper critical temperature)WithheldWithheld
Ms (martensite start)WithheldWithheld

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

D2

Foil wrap and a proper soak of 30 to 45 minutes matter at these temperatures. Tempering near 520 C trades a little hardness for secondary carbides and is the route to take before coating. Cold treatment reduces retained austenite.

M2

Needs staged preheats on the way up and a triple temper on the way down; the hardness comes from secondary carbides, not the quench alone. Strictly a professional-furnace steel.

Questions

What is the difference between D2 and M2 steel?
D2 carries more carbon: 1.4 to 1.6% against 0.78 to 0.88% in M2. M2 is alloyed with tungsten (5.5 to 6.75%), which D2 does not have in any real amount.
Is D2 or M2 harder after heat treatment?
Typical hardness for D2: 59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C. For M2: 63 to 66 HRC after triple tempering. The result depends on the temper you choose.
Can I heat treat D2 and M2 the same way?
No, each has its own recipe. D2: austenitize at 1000 to 1030 °C, quench in air, plates, or vacuum gas quench, temper at 200 to 530 °C. M2: austenitize at 1180 to 1220 °C, quench in salt bath, oil, or vacuum gas quench, temper at 540 to 570 °C.

Heat treatment numbers for your own steel, with sources.

Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat

Get HeatTreat on Google Play