Skip to content

AEB-L vs MagnaCut steel

AEB-L (Martensitic stainless steel). Razor-blade stainless: fine carbides, high hardness, and shocking toughness for the price.

MagnaCut (Powder-metallurgy stainless steel). The modern knife stainless designed to drop chromium carbide entirely: tough, hard, and truly rust resistant at once.

How AEB-L and MagnaCut differ

  • MagnaCut carries more carbon: 1.15% against 0.67% in AEB-L.
  • MagnaCut is alloyed with vanadium (4%), molybdenum (2%) and niobium (2%), which AEB-L does not have in any real amount.
  • AEB-L has far more chromium: 12.8% against 10.7%.
  • MagnaCut is austenitized hotter: 1065 to 1120 °C (1950 to 2050 °F) against 1050 to 1080 °C (1920 to 1975 °F) for AEB-L.
  • The quench differs. AEB-L: aluminium plates with forced air, then cold treatment. MagnaCut: aluminium plates, then cold treatment.

Side by side

AEB-L and MagnaCut compared
AEB-LMagnaCut
TypeMartensitic stainless steelPowder-metallurgy stainless steel
Carbon (C), wt %0.671.15
Manganese (Mn), wt %0.6none listed
Silicon (Si), wt %0.4none listed
Chromium (Cr), wt %12.810.7
Vanadium (V), wt %none listed4
Molybdenum (Mo), wt %none listed2
Niobium (Nb), wt %none listed2
Nitrogen (N), wt %none listed0.2
Austenitize1050 to 1080 °C (1920 to 1975 °F)1065 to 1120 °C (1950 to 2050 °F)
QuenchAluminium plates with forced air, then cold treatmentAluminium plates, then cold treatment
Temper150 to 200 °C (300 to 390 °F)150 to 175 °C (300 to 345 °F)
Typical hardness60 to 63 HRC with cold treatment60 to 64 HRC
Ac1 (lower critical temperature)WithheldWithheld
Ac3 (upper critical temperature)WithheldWithheld
Ms (martensite start)WithheldWithheld

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

AEB-L

The composition is balanced so nearly all carbide dissolves, so soak times are short, about 10 to 15 minutes, and the cold treatment genuinely matters for reaching full hardness.

MagnaCut

Cold treatment is close to mandatory at the higher austenitizing temperatures. The designer's published datasheet recommends keeping tempers at or below about 370 C to preserve corrosion resistance.

Questions

What is the difference between AEB-L and MagnaCut steel?
MagnaCut carries more carbon: 1.15% against 0.67% in AEB-L. MagnaCut is alloyed with vanadium (4%), molybdenum (2%) and niobium (2%), which AEB-L does not have in any real amount.
Is AEB-L or MagnaCut harder after heat treatment?
Typical hardness for AEB-L: 60 to 63 HRC with cold treatment. For MagnaCut: 60 to 64 HRC. The result depends on the temper you choose.
Can I heat treat AEB-L and MagnaCut the same way?
No, each has its own recipe. AEB-L: austenitize at 1050 to 1080 °C, quench in aluminium plates with forced air, then cold treatment, temper at 150 to 200 °C. MagnaCut: austenitize at 1065 to 1120 °C, quench in aluminium plates, then cold treatment, temper at 150 to 175 °C.