154CM steel heat treatment
The benchmark mid-range knife stainless: 440C's edge holding with better hot hardness from molybdenum. Typical practice for 154CM: austenitize at 1050 to 1095 °C (1920 to 2005 °F), quench (plates or oil, then cold treatment), then temper at 150 to 230 °C (300 to 445 °F).
- Austenitize
- 1050 to 1095 °C
- 1920 to 2005 °F
- Temper
- 150 to 230 °C
- 300 to 445 °F
- Quench
- Plates or oil, then cold treatment
- Typical hardness
- 59 to 62 HRC
Double temper. The powder-metallurgy version, CPM 154, has the same chemistry with finer carbides and is the better choice where toughness matters.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
154CM chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 1.05 |
| Manganese | Mn | 0.5 |
| Silicon | Si | 0.3 |
| Chromium | Cr | 14 |
| Molybdenum | Mo | 4 |
These are the producer's typical values, not a standard range. Martensitic stainless steel. Also known as: CPM 154 (PM version), ATS-34 (near).
154CM critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | Withheld | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | Withheld | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | Withheld | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Chromium near 14.0% puts 154CM outside the low-alloy steels these correlations were fitted to. High-chromium tool and stainless steels need measured data.
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 154CM steel at?
- Austenitize 154CM at 1050 to 1095 °C (1920 to 2005 °F), then quench: plates or oil, then cold treatment. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 154CM at?
- Temper 154CM at 150 to 230 °C (300 to 445 °F). Typical hardness: 59 to 62 HRC.
- What do you quench 154CM steel in?
- Plates or oil, then cold treatment. Double temper. The powder-metallurgy version, CPM 154, has the same chemistry with finer carbides and is the better choice where toughness matters.
- What is 154CM steel equivalent to?
- Other designations for 154CM, or for its nearest equivalent where marked "near": CPM 154 (PM version), ATS-34 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other stainless steels
- 420Martensitic stainless steel
- 440CMartensitic stainless steel
- AEB-LMartensitic stainless steel
- MagnaCutPowder-metallurgy stainless steel
Sources for this grade: Producer datasheet (typical values); Typical published practice.
Enter your own composition and get the numbers, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat