80CrV2 steel heat treatment
European chopper steel: 1080 with a little chromium and vanadium for deeper hardening and finer grain. Typical practice for 80CrV2: austenitize at 800 to 840 °C (1470 to 1545 °F), quench (fast oil), then temper at 175 to 230 °C (345 to 445 °F).
- Austenitize
- 800 to 840 °C
- 1470 to 1545 °F
- Temper
- 175 to 230 °C
- 345 to 445 °F
- Quench
- Fast oil
- Typical hardness
- 56 to 60 HRC after a 200 C temper
Handles thicker blades than plain 1080 thanks to the chromium. The vanadium keeps grain fine even with forge heats that wander hot.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
80CrV2 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.75 to 0.85 |
| Manganese | Mn | 0.3 to 0.5 |
| Silicon | Si | 0.15 to 0.35 |
| Chromium | Cr | 0.4 to 0.6 |
| Vanadium | V | 0.15 to 0.25 |
These are the producer's typical values, not a standard range. Cr-V high carbon steel. Also known as: 1.2235, L2 (near).
80CrV2 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 734 °C (1354 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 760 °C (1401 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 182 °C (360 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 80CrV2 steel at?
- Austenitize 80CrV2 at 800 to 840 °C (1470 to 1545 °F), then quench: fast oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 80CrV2 at?
- Temper 80CrV2 at 175 to 230 °C (345 to 445 °F). Typical hardness: 56 to 60 HRC after a 200 C temper.
- What do you quench 80CrV2 steel in?
- Fast oil. Handles thicker blades than plain 1080 thanks to the chromium. The vanadium keeps grain fine even with forge heats that wander hot.
- What is 80CrV2 steel equivalent to?
- Other designations for 80CrV2, or for its nearest equivalent where marked "near": 1.2235, L2 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other alloy steels
- 4130Cr-Mo alloy steel
- 4140Cr-Mo alloy steel
- 4340Ni-Cr-Mo alloy steel
- 5160Cr spring steel
- 6150Cr-V spring steel
- 8620Case-hardening alloy steel
- 9260Si-Mn spring steel
- 9310Case-hardening alloy steel
- 52100Bearing steel
- 300MUltra-high-strength steel
Sources for this grade: Producer datasheets (typical values); Typical published practice.
Enter your own composition and get the numbers, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat