154CM vs 440C steel
154CM (Martensitic stainless steel). The benchmark mid-range knife stainless: 440C's edge holding with better hot hardness from molybdenum.
440C (Martensitic stainless steel). The classic high-hardness stainless for bearings, valve seats and knives that must not rust.
How 154CM and 440C differ
- Carbon is close: 1.05% in 154CM and 0.95 to 1.2% in 440C.
- 440C has far more chromium: 16 to 18% against 14%.
- 154CM is austenitized hotter: 1050 to 1095 °C (1920 to 2005 °F) against 1010 to 1065 °C (1850 to 1950 °F) for 440C.
- The quench differs. 154CM: plates or oil, then cold treatment. 440C: air, plates, or oil.
Side by side
| 154CM | 440C | |
|---|---|---|
| Type | Martensitic stainless steel | Martensitic stainless steel |
| Carbon (C), wt % | 1.05 | 0.95 to 1.2 |
| Manganese (Mn), wt % | 0.5 | 1 max |
| Silicon (Si), wt % | 0.3 | 1 max |
| Chromium (Cr), wt % | 14 | 16 to 18 |
| Molybdenum (Mo), wt % | 4 | 0.75 max |
| Austenitize | 1050 to 1095 °C (1920 to 2005 °F) | 1010 to 1065 °C (1850 to 1950 °F) |
| Quench | Plates or oil, then cold treatment | Air, plates, or oil |
| Temper | 150 to 230 °C (300 to 445 °F) | 150 to 230 °C (300 to 445 °F) |
| Typical hardness | 59 to 62 HRC | 57 to 60 HRC |
| Ac1 (lower critical temperature) | Withheld | Withheld |
| Ac3 (upper critical temperature) | Withheld | Withheld |
| Ms (martensite start) | Withheld | Withheld |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
154CM
Double temper. The powder-metallurgy version, CPM 154, has the same chemistry with finer carbides and is the better choice where toughness matters.
440C
Cold treatment after the quench is common to convert retained austenite. Avoid tempering between about 425 and 565 C, where corrosion resistance and toughness both fall.
Questions
- What is the difference between 154CM and 440C steel?
- Carbon is close: 1.05% in 154CM and 0.95 to 1.2% in 440C. 440C has far more chromium: 16 to 18% against 14%.
- Is 154CM or 440C harder after heat treatment?
- Typical hardness for 154CM: 59 to 62 HRC. For 440C: 57 to 60 HRC. The result depends on the temper you choose.
- Can I heat treat 154CM and 440C the same way?
- No, each has its own recipe. 154CM: austenitize at 1050 to 1095 °C, quench in plates or oil, then cold treatment, temper at 150 to 230 °C. 440C: austenitize at 1010 to 1065 °C, quench in air, plates, or oil, temper at 150 to 230 °C.
Heat treatment numbers for your own steel, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat