Skip to content

80CrV2 vs 52100 steel

80CrV2 (Cr-V high carbon steel). European chopper steel: 1080 with a little chromium and vanadium for deeper hardening and finer grain.

52100 (Bearing steel). Ball-bearing steel, and one of the finest fine-edge knife steels when heat treated with care.

How 80CrV2 and 52100 differ

  • 52100 carries more carbon: 0.98 to 1.1% against 0.75 to 0.85% in 80CrV2.
  • 52100 is austenitized hotter: 840 to 860 °C (1545 to 1580 °F) against 800 to 840 °C (1470 to 1545 °F) for 80CrV2.
  • The quench differs. 80CrV2: fast oil. 52100: oil.

Side by side

80CrV2 and 52100 compared
80CrV252100
TypeCr-V high carbon steelBearing steel
Carbon (C), wt %0.75 to 0.850.98 to 1.1
Manganese (Mn), wt %0.3 to 0.50.25 to 0.45
Silicon (Si), wt %0.15 to 0.350.15 to 0.35
Chromium (Cr), wt %0.4 to 0.61.3 to 1.6
Vanadium (V), wt %0.15 to 0.25none listed
Austenitize800 to 840 °C (1470 to 1545 °F)840 to 860 °C (1545 to 1580 °F)
QuenchFast oilOil
Temper175 to 230 °C (345 to 445 °F)160 to 230 °C (320 to 445 °F)
Typical hardness56 to 60 HRC after a 200 C temper58 to 64 HRC depending on temper
Ac1 (lower critical temperature)about 734 °C (1354 °F)about 751 °C (1384 °F)
Ac3 (upper critical temperature)about 760 °C (1401 °F)Withheld
Ms (martensite start)about 182 °C (360 °F)about 71 °C (160 °F)

Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

Heat treating each one

80CrV2

Handles thicker blades than plain 1080 thanks to the chromium. The vanadium keeps grain fine even with forge heats that wander hot.

52100

Harden from the spheroidized condition with a modest soak of 10 to 20 minutes. Hypereutectoid, so the right austenitizing dissolves only part of the carbide. Cold treatment can cut retained austenite when maximum stability matters.

Questions

What is the difference between 80CrV2 and 52100 steel?
52100 carries more carbon: 0.98 to 1.1% against 0.75 to 0.85% in 80CrV2. 52100 is austenitized hotter: 840 to 860 °C (1545 to 1580 °F) against 800 to 840 °C (1470 to 1545 °F) for 80CrV2.
Is 80CrV2 or 52100 harder after heat treatment?
Typical hardness for 80CrV2: 56 to 60 HRC after a 200 C temper. For 52100: 58 to 64 HRC depending on temper. The result depends on the temper you choose.
Can I heat treat 80CrV2 and 52100 the same way?
No, each has its own recipe. 80CrV2: austenitize at 800 to 840 °C, quench in fast oil, temper at 175 to 230 °C. 52100: austenitize at 840 to 860 °C, quench in oil, temper at 160 to 230 °C.

Heat treatment numbers for your own steel, with sources.

Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat