MagnaCut steel heat treatment
The modern knife stainless designed to drop chromium carbide entirely: tough, hard, and truly rust resistant at once. Typical practice for CPM MagnaCut: austenitize at 1065 to 1120 °C (1950 to 2050 °F), quench (aluminium plates, then cold treatment), then temper at 150 to 175 °C (300 to 345 °F).
- Austenitize
- 1065 to 1120 °C
- 1950 to 2050 °F
- Temper
- 150 to 175 °C
- 300 to 345 °F
- Quench
- Aluminium plates, then cold treatment
- Typical hardness
- 60 to 64 HRC
Cold treatment is close to mandatory at the higher austenitizing temperatures. The designer's published datasheet recommends keeping tempers at or below about 370 C to preserve corrosion resistance.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
MagnaCut chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 1.15 |
| Chromium | Cr | 10.7 |
| Vanadium | V | 4 |
| Molybdenum | Mo | 2 |
| Niobium | Nb | 2 |
| Nitrogen | N | 0.2 |
These are the producer's typical values, not a standard range. Powder-metallurgy stainless steel.
MagnaCut critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | Withheld | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | Withheld | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | Withheld | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Chromium near 10.7% puts MagnaCut outside the low-alloy steels these correlations were fitted to. High-chromium tool and stainless steels need measured data.
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden MagnaCut steel at?
- Austenitize MagnaCut at 1065 to 1120 °C (1950 to 2050 °F), then quench: aluminium plates, then cold treatment. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper MagnaCut at?
- Temper MagnaCut at 150 to 175 °C (300 to 345 °F). Typical hardness: 60 to 64 HRC.
- What do you quench MagnaCut steel in?
- Aluminium plates, then cold treatment. Cold treatment is close to mandatory at the higher austenitizing temperatures. The designer's published datasheet recommends keeping tempers at or below about 370 C to preserve corrosion resistance.
Other stainless steels
- 420Martensitic stainless steel
- 440CMartensitic stainless steel
- AEB-LMartensitic stainless steel
- 154CMMartensitic stainless steel
Sources for this grade: Producer datasheet (typical values); Typical published practice.