Skip to content

AEB-L steel heat treatment

Razor-blade stainless: fine carbides, high hardness, and shocking toughness for the price. Typical practice for AEB-L: austenitize at 1050 to 1080 °C (1920 to 1975 °F), quench (aluminium plates with forced air, then cold treatment), then temper at 150 to 200 °C (300 to 390 °F).

Austenitize
1050 to 1080 °C
1920 to 1975 °F
Temper
150 to 200 °C
300 to 390 °F
Quench
Aluminium plates with forced air, then cold treatment
Typical hardness
60 to 63 HRC with cold treatment

The composition is balanced so nearly all carbide dissolves, so soak times are short, about 10 to 15 minutes, and the cold treatment genuinely matters for reaching full hardness.

Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.

AEB-L chemical composition

AEB-L chemical composition in weight per cent
ElementSymbolWeight %
CarbonC0.67
ManganeseMn0.6
SiliconSi0.4
ChromiumCr12.8

These are the producer's typical values, not a standard range. Martensitic stainless steel. Also known as: 13C26 (near).

AEB-L critical temperatures

Estimated critical temperatures for AEB-L
TemperatureWhat it meansEstimateEquation
Ac1Lower critical temperatureWithheldAc1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W
Ac3Upper critical temperatureWithheldAc3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W
MsMartensite startWithheldMs = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo

Chromium near 12.8% puts AEB-L outside the low-alloy steels these correlations were fitted to. High-chromium tool and stainless steels need measured data.

Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.

Questions

What temperature do you harden AEB-L steel at?
Austenitize AEB-L at 1050 to 1080 °C (1920 to 1975 °F), then quench: aluminium plates with forced air, then cold treatment. This is typical published practice; section size and furnace accuracy shift the right number.
What temperature do you temper AEB-L at?
Temper AEB-L at 150 to 200 °C (300 to 390 °F). Typical hardness: 60 to 63 HRC with cold treatment.
What do you quench AEB-L steel in?
Aluminium plates with forced air, then cold treatment. The composition is balanced so nearly all carbide dissolves, so soak times are short, about 10 to 15 minutes, and the cold treatment genuinely matters for reaching full hardness.
What is AEB-L steel equivalent to?
Other designations for AEB-L, or for its nearest equivalent where marked "near": 13C26 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.

Other stainless steels

Enter your own composition and get the numbers, with sources.

Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat