O1 vs A2 steel
O1 (Oil-hardening tool steel). The gauge-plate standard. Predictable, fine grained, and at home in every tool room and knife shop.
A2 (Air-hardening tool steel). Air-hardening die steel: the stability of a gas quench with real wear resistance. A fine hard-use knife steel.
How O1 and A2 differ
- A2 carries more carbon: 0.95 to 1.05% against 0.85 to 1% in O1.
- O1 is alloyed with tungsten (0.4 to 0.6%), which A2 does not have in any real amount.
- A2 is alloyed with molybdenum (0.9 to 1.4%) and vanadium (0.15 to 0.5%), which O1 does not have in any real amount.
- A2 has far more chromium: 4.75 to 5.5% against 0.4 to 0.6%.
- A2 is austenitized hotter: 925 to 980 °C (1695 to 1795 °F) against 790 to 815 °C (1455 to 1500 °F) for O1.
- The quench differs. O1: oil. A2: still air or aluminium plates.
Side by side
| O1 | A2 | |
|---|---|---|
| Type | Oil-hardening tool steel | Air-hardening tool steel |
| Carbon (C), wt % | 0.85 to 1 | 0.95 to 1.05 |
| Manganese (Mn), wt % | 1 to 1.4 | 1 max |
| Silicon (Si), wt % | 0.5 max | 0.5 max |
| Chromium (Cr), wt % | 0.4 to 0.6 | 4.75 to 5.5 |
| Tungsten (W), wt % | 0.4 to 0.6 | none listed |
| Vanadium (V), wt % | 0.3 max | 0.15 to 0.5 |
| Molybdenum (Mo), wt % | none listed | 0.9 to 1.4 |
| Austenitize | 790 to 815 °C (1455 to 1500 °F) | 925 to 980 °C (1695 to 1795 °F) |
| Quench | Oil | Still air or aluminium plates |
| Temper | 150 to 260 °C (300 to 500 °F) | 175 to 230 °C (345 to 445 °F) |
| Typical hardness | 57 to 64 HRC depending on temper | 57 to 62 HRC |
| Ac1 (lower critical temperature) | about 729 °C (1344 °F) | Withheld |
| Ac3 (upper critical temperature) | Withheld | Withheld |
| Ms (martensite start) | about 105 °C (221 °F) | Withheld |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
O1
Soak 10 to 20 minutes at temperature. Moves little in the quench, which is why gauge makers standardized on it. Anneal at 760 to 790 C with a slow cool when you need to re-machine.
A2
Wrap in stainless foil against decarburization, soak 20 to 45 minutes, cool in still air. Double tempering is standard practice. Distortion is low enough to harden finished parts.
Questions
- What is the difference between O1 and A2 steel?
- A2 carries more carbon: 0.95 to 1.05% against 0.85 to 1% in O1. O1 is alloyed with tungsten (0.4 to 0.6%), which A2 does not have in any real amount.
- Is O1 or A2 harder after heat treatment?
- Typical hardness for O1: 57 to 64 HRC depending on temper. For A2: 57 to 62 HRC. The result depends on the temper you choose.
- Can I heat treat O1 and A2 the same way?
- No, each has its own recipe. O1: austenitize at 790 to 815 °C, quench in oil, temper at 150 to 260 °C. A2: austenitize at 925 to 980 °C, quench in still air or aluminium plates, temper at 175 to 230 °C.
Heat treatment numbers for your own steel, with sources.