D2 vs S7 steel
D2 (High-carbon high-chromium tool steel). The blanking-die classic: huge carbide volume, high wear resistance, semi-stainless behavior.
S7 (Shock-resisting tool steel). The jackhammer-bit steel: built to take impact at 54 to 57 HRC without shattering.
How D2 and S7 differ
- D2 carries more carbon: 1.4 to 1.6% against 0.45 to 0.55% in S7.
- D2 is alloyed with vanadium (1.1 max%), which S7 does not have in any real amount.
- D2 has far more chromium: 11 to 13% against 3 to 3.5%.
- D2 is austenitized hotter: 1000 to 1030 °C (1830 to 1885 °F) against 925 to 955 °C (1695 to 1750 °F) for S7.
- The quench differs. D2: air, plates, or vacuum gas quench. S7: air up to about 60 mm, otherwise interrupted oil.
Side by side
| D2 | S7 | |
|---|---|---|
| Type | High-carbon high-chromium tool steel | Shock-resisting tool steel |
| Carbon (C), wt % | 1.4 to 1.6 | 0.45 to 0.55 |
| Manganese (Mn), wt % | 0.6 max | 0.2 to 0.9 |
| Silicon (Si), wt % | 0.6 max | 0.2 to 1 |
| Chromium (Cr), wt % | 11 to 13 | 3 to 3.5 |
| Molybdenum (Mo), wt % | 0.7 to 1.2 | 1.3 to 1.8 |
| Vanadium (V), wt % | 1.1 max | none listed |
| Austenitize | 1000 to 1030 °C (1830 to 1885 °F) | 925 to 955 °C (1695 to 1750 °F) |
| Quench | Air, plates, or vacuum gas quench | Air up to about 60 mm, otherwise interrupted oil |
| Temper | 200 to 530 °C (390 to 985 °F) | 205 to 540 °C (400 to 1005 °F) |
| Typical hardness | 59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C | 54 to 57 HRC at a 205 C temper |
| Ac1 (lower critical temperature) | Withheld | about 790 °C (1453 °F) |
| Ac3 (upper critical temperature) | Withheld | about 842 °C (1548 °F) |
| Ms (martensite start) | Withheld | about 260 °C (500 °F) |
Ac1, Ac3 and Ms are estimates from the Andrews (1965) correlations at mid-range composition. They are withheld where a steel falls outside the low-alloy range those correlations cover, and Ac3 is withheld for steels above about 0.8% carbon. Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
Heat treating each one
D2
Foil wrap and a proper soak of 30 to 45 minutes matter at these temperatures. Tempering near 520 C trades a little hardness for secondary carbides and is the route to take before coating. Cold treatment reduces retained austenite.
S7
Air hardening in most sections, which keeps distortion down on chisels and punches. Temper immediately after the quench; shock steels resent waiting around untempered.
Questions
- What is the difference between D2 and S7 steel?
- D2 carries more carbon: 1.4 to 1.6% against 0.45 to 0.55% in S7. D2 is alloyed with vanadium (1.1 max%), which S7 does not have in any real amount.
- Is D2 or S7 harder after heat treatment?
- Typical hardness for D2: 59 to 61 HRC with a 200 C temper, 56 to 58 HRC double tempered near 520 C. For S7: 54 to 57 HRC at a 205 C temper. The result depends on the temper you choose.
- Can I heat treat D2 and S7 the same way?
- No, each has its own recipe. D2: austenitize at 1000 to 1030 °C, quench in air, plates, or vacuum gas quench, temper at 200 to 530 °C. S7: austenitize at 925 to 955 °C, quench in air up to about 60 mm, otherwise interrupted oil, temper at 205 to 540 °C.
Heat treatment numbers for your own steel, with sources.
Heat treatment numbers for common steels, each traced to its source paper. About HeatTreat