9260 steel heat treatment
Silicon spring steel with legendary flex. A favorite for swords that must survive abuse. Typical practice for AISI 9260: austenitize at 815 to 870 °C (1500 to 1600 °F), quench (oil), then temper at 190 to 480 °C (375 to 895 °F).
- Austenitize
- 815 to 870 °C
- 1500 to 1600 °F
- Temper
- 190 to 480 °C
- 375 to 895 °F
- Quench
- Oil
- Typical hardness
- 57 to 59 HRC at a 200 C temper, 45 to 50 HRC at spring tempers
Silicon strengthens the ferrite and resists tempering, so it holds hardness at higher tempers than plain carbon steel. Decarburization in the forge is the thing to watch: silicon steels lose surface carbon quickly.
Typical published practice for guidance. Section size, prior condition, furnace accuracy and soak time all shift the right numbers. Verify against your steel supplier's datasheet before hardening anything that matters.
9260 chemical composition
| Element | Symbol | Weight % |
|---|---|---|
| Carbon | C | 0.56 to 0.64 |
| Manganese | Mn | 0.75 to 1 |
| Silicon | Si | 1.8 to 2.2 |
These are the limits of the standard's chemical range. Si-Mn spring steel. Also known as: 60SiMn5 (near), 1.5028 (near).
9260 critical temperatures
| Temperature | What it means | Estimate | Equation |
|---|---|---|---|
| Ac1 | Lower critical temperature | about 772 °C (1421 °F) | Ac1 = 723 - 10.7 Mn - 16.9 Ni + 29.1 Si + 16.9 Cr + 6.38 W |
| Ac3 | Upper critical temperature | about 842 °C (1548 °F) | Ac3 = 910 - 203 sqrt(C) + 44.7 Si - 15.2 Ni + 31.5 Mo + 104 V + 13.1 W |
| Ms | Martensite start | about 259 °C (497 °F) | Ms = 539 - 423 C - 30.4 Mn - 17.7 Ni - 12.1 Cr - 7.5 Mo |
Estimates from the mid-range composition, with element amounts in weight per cent. Correlations like these scatter by about 20 to 25 °C against measurement, and real values shift with heating rate. Source: K.W. Andrews, "Empirical formulae for the calculation of some transformation temperatures", Journal of the Iron and Steel Institute, 203 (1965) 721-727.
Questions
- What temperature do you harden 9260 steel at?
- Austenitize 9260 at 815 to 870 °C (1500 to 1600 °F), then quench: oil. This is typical published practice; section size and furnace accuracy shift the right number.
- What temperature do you temper 9260 at?
- Temper 9260 at 190 to 480 °C (375 to 895 °F). Typical hardness: 57 to 59 HRC at a 200 C temper, 45 to 50 HRC at spring tempers.
- What do you quench 9260 steel in?
- Oil. Silicon strengthens the ferrite and resists tempering, so it holds hardness at higher tempers than plain carbon steel. Decarburization in the forge is the thing to watch: silicon steels lose surface carbon quickly.
- What is 9260 steel equivalent to?
- Other designations for 9260, or for its nearest equivalent where marked "near": 60SiMn5 (near), 1.5028 (near). Check the chemistry on your supplier's datasheet before treating them as the same steel.
Other alloy steels
- 4130Cr-Mo alloy steel
- 4140Cr-Mo alloy steel
- 4340Ni-Cr-Mo alloy steel
- 5160Cr spring steel
- 6150Cr-V spring steel
- 8620Case-hardening alloy steel
- 9310Case-hardening alloy steel
- 52100Bearing steel
- 80CrV2Cr-V high carbon steel
- 300MUltra-high-strength steel
Sources for this grade: SAE J404 chemical ranges; Typical published practice.
Enter your own composition and get the numbers, with sources.